Fabrication of GaN mesa structures

Published online by Cambridge University Press:  13 June 2014

K.V. Vassilevski
Affiliation:
Cree Research EED
M.G. Rastegaeva
Affiliation:
Ioffe Physical-Technical Institute
A.I. Babanin
Affiliation:
Cree Research EED and Ioffe Physical-Technical Institute
I.P. Nikitina
Affiliation:
Cree Research EED and Ioffe Physical-Technical Institute
V.A. Dmitriev
Affiliation:
Cree Research EED and Ioffe Physical-Technical Institute

Abstract

We report on nickel based technology for the fabrication of GaN mesa structures. Ti/Ni ohmic contacts for n-doped GaN with contact resistivity Rc ~2×10−5  Ω×cm2 and Ni ohmic contacts for p-doped GaN with Rc ~ 4×10−2 Ω×cm2 were formed. Both types of contacts were used as masks for GaN reactive ion etching (RIE) in a CCl2F2/Ar gas mixture. Maximum etch rates of ~ 40 nm/min were obtained. Mesa structures up to 3 μm in height were formed.

Type
Research Article
Copyright
Copyright © 1996 Materials Research Society

1. Introduction

GaN and related Al(In)xGa1−xN solid solutions are wide band gap materials which are promising for a variety of applications such as laser diodes Reference Nakamura, Senoh, Nagahama, Iwasa, Yamada, Matsushita, Kiyoku and Sugimoto[1], light emitting diodes Reference Kong, Leonard, Bulman and Edmond[2], microwave and high temperature devices Reference Morkoc, Strite, Gao, Lin, Sverdlov and Burns[3] Reference Chelnokov, Vassilevski, Dmitriev, Prelas, Gielisse, Popovici, Spitsyn and Stacy[4]. To realize the great potential of III-V nitrides and to follow the recent progress in their epitaxial growth, especially by MOCVD Reference Dmitriev, Irvine and Edmond[5] and HVPE Reference Melnik, Nikitina, Zubrilov, Sitnikova, Musikhin and Dmitriev[6], it is necessary to develop the appropriate post-growth device fabrication technologies. Among other problems, the formation of ohmic contacts for n- and p-doped materials and RIE process are of the greatest importance. An additional requirement for these technological stages is their mutual compatibility in the process of device fabrication. The goal of this research was to find a metallization suitable for self-aligned technology so the ohmic contact could be used as a mask for GaN RIE. or so that the mask could be used as a contact. Various metals have already been used to form contacts to GaN. Ti, Ti/Al and TiN Reference Brown, Ramer, Banas, Lester, Malloy and Hersee[7] Reference Smith, Bremser, Carlson, Weeks, Huang, Kim, Carpenter and Davis[8] Reference Wu, Jiang, Keller, Keller, Kapolnek, Denbaars and Mishra[9] Reference Lin, Ma, Huang, Fan, Allen and Morkoc[10] were utilized for n-GaN. TiN, Au, Au/Mg Reference Smith, Bremser, Carlson, Weeks, Huang, Kim, Carpenter and Davis[8], Cr/Au Reference Yoo, Shim, Myoung, Ping, Kim and Adesida[11] and Ni/Au Reference Nakamura, Yoshikawa, Kishino, Kobayashi and Yasuda[12] were used for p-GaN. We investigated Ni-based contacts, since Ni can be used as a mask for GaN plasma etching Reference Vassilevski, Sizov, Babanin, Melnik and Zubrilov[13], and as a Schottky barrier to n-GaN Reference Kalinina, Kuznetsov, Dmitriev, Irvine and Carter[14]. In addition, Ni is usually used to form an ohmic contact to 6H-SiC, which is a highly suitable substrate material for the epitaxial growth of GaN Reference Crofton, McMullin, Williams and Bozack[15] Reference Rastegaeva, Andreev, Chelnokov, Vassilevski, Babanin, Nikitina, Lavrent’ev and Udaltsov[16].

2. Ti/Ni ohmic contacts on n-doped GaN

2.1 Sample preparation and measurement techniques

1.5 μm thick GaN layers with a donor concentration of ~1 × 1018cm−3 were grown for this study on 6H-SiC substrates by MOCVD at Cree Research, Inc. To form the Ti/Ni contact, 50 nm thick Ti was deposited by e-beam sputtering on GaN at 350°C. After that, the Ti film was covered by a 250 nm thick Ni layer deposited at room temperature. After the contact pattern had been formed by photolithography, the samples were annealed in a nitrogen atmosphere at a pressure of 200 Torr and temperatures ranging from 300°C to 1150°C. The circular TLM (CTLM) technique was applied to measure the contact resistivity. The scheme of photomask used for CTLM is shown in Figure 1. The diameter of the inner dot contact (2r) was 40  μm and outer ring contact diameters (2R) varied from 100 to 500 μm. The composition of the metal both before and after annealing was measured by Auger electron spectroscopy (AES) and X-ray diffraction (XRD).

Figure 1. The Rtot dependence of ln(R/r) for Ti/Ni contact on n-GaN after annealing for 30 sec at 1040°C. The scheme of pattern used for contact resistivity measurements is shown in the inset. The black regions are covered by metal.

2.2 Experimental results

Annealing at temperatures lower than 950°C only resulted in Ti diffusion towards the surface of the sample (Figure 2). In addition to Ti diffusion, an interaction between Ni and GaN was observed after annealing at temperatures above 950°C. The formation of a Ga2Ni3 phase was observed by XRD. The content of Ga2Ni3 decreased sharply after annealing at temperatures above 1050°C. Linear current voltage (I-V) characteristics for the contact were observed after annealing at temperatures above 950°C. The contact with the lowest value of Rc= 1.1 × 10−5Ωcm2 was formed after annealing for 30 sec at 1040°C. No contact degradation was observed up to dc current densities of 30 kA/cm2. Figure 1 presents the dependence of total resistance Rtot on ln(R/r) measured for this sample at room temperature. Although the formation of ohmic contacts at high temperature was caused mainly by the interaction of Ni with GaN, the Ti also played an important role in this process. The diffusion of Ti through the nickel cap layer was accompanied by the removal of oxygen from the metal-nitride interface as shown in Figure 2.

Figure 2. The AES profiles of Ti/Ni contacts: (1) as deposited; (2) annealed at 600°C for 300 sec; (3) annealed at 950°C for 140 sec; and (4) annealed at 1040°C for 140 sec.

The change of GaN bulk electronic properties caused by the temperature treatments was monitored by measuring the sheet resistivity Rs. Rs did not increase substantially after annealing at temperatures below 1050°C. Further increase in the temperature led to a simultaneous increase in Rc and Rs (Rc= 2 × 10−5Ωcm2; Rs= 85 Ω/sq after annealing for 140 sec at 1050°C and Rc= 2 × 10−4Ωcm2; Rs= 140 Ω/sq after annealing for 30 sec at 1150°C).

3. RIE of GaN

Dry etching of III-V nitrides in chloride based plasmas by the RIE technique Reference Lin, Fan, Ma, Allen and Morkoc[17] Reference Ping, Adesida and Khan[18] Reference Adesida, Mahajan, Andideh, Asif Khan, Olsen and Kuznia[19], the electron cyclotron resonance discharge technique Reference Pearton, Abernathy, Ren, Lothian, Wisk and Katz[20] Reference Pearton, Abernathy and Ren[21] Reference Pearton, Abernathy and Ren[22], and chemically assisted ion beam etching Reference Ping, Youtsey and Adesida[23] Reference Ping, Adesida and Khan[24] has been reported.

We examined three RIE masking materials for GaN using a gas mixture containing CCl2F2 Reference Vassilevski, Sizov, Babanin, Melnik and Zubrilov[13]. They were: (1) 0.1 μm-thick Ni deposited by e-beam sputtering on the substrate heated to 350°C; (2) 0.2 μm-thick Ni deposited by thermal evaporation on the substrate heated to 550°C; and (3) the ohmic contact discussed above.

The plasma was generated by a radio frequency (13.56 MHz) discharge into a stainless steel/quartz reactor using induction plasma excitation (H-mode) and a maximum rf power of 5 kW. The reactor has a diameter of 17 cm and height 15 cm. A grounded electrode served as a substrate holder. The electrode was not cooled and its temperature during the etch was about 200°C. To avoid the deposition of a CFx-like film, we used Ar as a carrier gas. Single crystal GaN and AlGaN epitaxial layers up to 8 μm in thickness grown on the (0001)Si face of 6H-SiC Reference Dmitriev, Irvine and Edmond[5] Reference Dmitriev, Irvine, Carter, Zubrilov and Tsvetkov[25] were used to study the etch process.

The etch rates of both Ni masks were very low (<10 Å/min) under the RIE conditions used. Ti/Ni contact also demonstrated good chemical stability sufficient for the formation of 2 μm height mesa structures, in spite of the fact that the Ni layer was mixed with Ga through annealing. Furthermore, the as-deposited Ti/Ni metalization lifted off during the exposure in CCl2F2/Ar plasma, since Ti was etched through the edge of pattern.

Etch rates of GaN ranging from 60 Å/min to 400 Å/min were obtained depending on the pressure and gas flow rate. The etch rates for n-GaN and p-GaN were similar and did not depend on the Al content in AlxGa1−xN up to × = 0.15. The maximum GaN etch rate was about 400 Å/min at a pressure of 10 mTorr for a CCl2F2:Ar (12 sccm : 12 sccm) gas mixture. The SEM micrograph shown in Figure 3 demonstrates a cleaved GaN/SiC sample with a strip-like mesa structure formed by RIE. The height of mesa structure is 3.2 μm. The Ni mask deposited by e-beam sputtering is not removed. The surface of the GaN layer is smooth and free from contamination after etching. Both walls of the mesa structure are inclined at an angle about 60 degrees with respect to the surface. Two kinds of microrelief are clearly seen on mesa-structure side wall: (1) vertical peculiarities caused by the mask edge effect, and (2) uniformly spread hollows caused by the nature of RIE process.

Figure 3. The SEM micrograph of a cleaved GaN/SiC sample with a stripe-like mesa structure formed by RIE in CCl2F2:Ar (12 sccm : 12 sccm) at 10 mTorr. The Ni mask, deposited by e-beam sputtering, is not removed.

4. Ni mask as a contact to p-GaN

It was observed that the thermally evaporated Ni revealed almost linear I-V characteristic when was used as a masking material for RIE of p-GaN. To prove this fact, Ni was deposited on 0.5 μm thick p-GaN layer with Na-Nd concentration of about 1018cm−3 as was measured by Hg probe. After deposition, Ni was patterned for CTLM measurements. The contacts demonstrated symmetrical I-V characteristics with offset voltages less than 100 mV and linear I-V dependencies at higher voltages. Contacts were investigated at dc current densities up to 330 A/cm2. Contact resistance was estimated to be Rc= 4 × 10−2Ωcm2. Figure 4 presents the dependence of Rtot on ln(R/r) measured at current density of 33 A/cm2 and room temperature. In contrast, Ni deposited by e-beam sputtering did not reveal such a near linear I-V characteristic, even when annealed at temperature 550°C.

Figure 4. The Rtot dependence of ln(R/r) for Ni contact on p-GaN.

5. Conclusion

In summary, a Ni based technology suitable for the fabrication of GaN mesa structures was developed. The main achievements are: (1) Ti/Ni ohmic contacts with Rc ~ 2 × 10−5 Ωcm2 to n-GaN, (2) Ni contacts with Rc ~ 4 × 10−2 Ωcm2 to p-GaN, and (3) GaN RIE using gas mixture containing dichlor-difluoromethane; the above contacts serving as masks.

Acknowledgments

The authors would like to thank Dr. E. V. Kalinina for metal vacuum deposition and V. E. Sizov for technical assistance.

References

Nakamura, S, Senoh, M, Nagahama, S, Iwasa, N, Yamada, T, Matsushita, T, Kiyoku, H, Sugimoto, Y, Jpn. J. Appl. Phys. 35, L74-L76 (1996).CrossRefGoogle Scholar
Kong, KS, Leonard, M, Bulman, G, Edmond, J, unpublished (1996).Google Scholar
Morkoc, H., Strite, S., Gao, G. B., Lin, M. E., Sverdlov, B., Burns, M., J. Appl. Phys. 76, 1363-1398 (1994).CrossRefGoogle Scholar
Chelnokov, VE, Vassilevski, KV, Dmitriev, VA, in Wide Bandgap Electronic Materials, NATO ASI series, 3. High Technology, vol.1, Edited by: Prelas, MA, Gielisse, P, Popovici, G, Spitsyn, BV, Stacy, T, (Kluwer Academic Publishers, Dordrecht, 1995) 453-461.Google Scholar
Dmitriev, VA, Irvine, KG, Edmond, JA, et al., Inst. Phys. Conf. Ser. 141, 497-502 (1995).Google Scholar
Melnik, YuV, Nikitina, IP, Zubrilov, AS, Sitnikova, AA, Musikhin, YuG, Dmitriev, VA, Inst. Phys. Conf. Ser. 142, 863-866 (1996).Google Scholar
Brown, J, Ramer, J, Banas, M, Lester, LF, Malloy, KJ, Hersee, SD, unpublished (1996).Google Scholar
Smith, LL, Bremser, MD, Carlson, EP, Weeks, TW, Huang, Y, Kim, MJ, Carpenter, RW, Davis, RF, unpublished (1996).Google Scholar
Wu, Y, Jiang, W, Keller, B, Keller, S, Kapolnek, D, Denbaars, S, Mishra, U, unpublished (1996).Google Scholar
Lin, M. E., Ma, Z., Huang, F. Y., Fan, Z. F., Allen, L. H., Morkoc, H., Appl. Phys. Lett. 64, 1003-1005 (1994).CrossRefGoogle Scholar
Yoo, MC, Shim, KH, Myoung, JM, Ping, AT, Kim, K, Adesida, I, unpublished (1996).Google Scholar
Nakamura, S, in Proc. of Int. Symposium on Blue Laser and Light Emitting Diodes, Edited by: Yoshikawa, A, Kishino, K, Kobayashi, M, Yasuda, T, (Chiba University, Chiba, 1996) 119-123.Google Scholar
Vassilevski, KV, Sizov, VE, Babanin, AI, Melnik, YuV, Zubrilov, AS, Inst. Phys. Conf. Ser. 142, 1027-1030 (1996).Google Scholar
Kalinina, EV, Kuznetsov, NI, Dmitriev, VA, Irvine, KG, Carter, CH, J. Electron. Mater. 25, 831-834 (1996).CrossRefGoogle Scholar
Crofton, J, McMullin, PG, Williams, JR, Bozack, MJ, J. Appl. Phys. 77, 1317-1319 (1995).CrossRefGoogle Scholar
Rastegaeva, MG, Andreev, AN, Chelnokov, VE, Vassilevski, KV, Babanin, AI, Nikitina, IP, Lavrent’ev, AA, in Int. Seminar Semiconductor Silicon Carbide and SiC-Based Devices, Book of of Abstracts, Edited by: Udaltsov, VE, (Novgorod State University, Novgorod, 1995) 50-52.Google Scholar
Lin, M. E., Fan, Z. F., Ma, Z., Allen, L. H., Morkoc, H., Appl. Phys. Lett. 64, 887-888 (1994).CrossRefGoogle Scholar
Ping, AT, Adesida, I, Khan, MA, et al., Electron. Lett. 30, 1895-1897 (1994).CrossRefGoogle Scholar
Adesida, I., Mahajan, A., Andideh, E., Asif Khan, M., Olsen, D. T., Kuznia, J. N., Appl. Phys. Lett. 63, 2777-2779 (1993).CrossRefGoogle Scholar
Pearton, S. J., Abernathy, C. R., Ren, F., Lothian, J. R., Wisk, P. W., Katz, A., J. Vac. Sci. Technol. A 11, 1772-1775 (1993).CrossRefGoogle Scholar
Pearton, S. J., Abernathy, C. R., Ren, F., Appl. Phys. Lett. 64, 2294-2296 (1994).CrossRefGoogle Scholar
Pearton, S. J., Abernathy, C. R., Ren, F., Appl. Phys. Lett. 64, 3643-3645 (1994).CrossRefGoogle Scholar
Ping, AT, Youtsey, C, Adesida, I, et al., J. Electron. Mater. 24, 229-234 (1995).CrossRefGoogle Scholar
Ping, A. T., Adesida, I., Khan, M. Asif, Appl. Phys. Lett. 67, 1250-1252 (1995).CrossRefGoogle Scholar
Dmitriev, V. A., Irvine, K., Carter, C. H. Jr. Zubrilov, A. S., Tsvetkov, D. V., Appl. Phys. Lett. 67, 115-117 (1995).CrossRefGoogle Scholar
Figure 0

Figure 1. The Rtot dependence of ln(R/r) for Ti/Ni contact on n-GaN after annealing for 30 sec at 1040°C. The scheme of pattern used for contact resistivity measurements is shown in the inset. The black regions are covered by metal.

Figure 1

Figure 2. The AES profiles of Ti/Ni contacts: (1) as deposited; (2) annealed at 600°C for 300 sec; (3) annealed at 950°C for 140 sec; and (4) annealed at 1040°C for 140 sec.

Figure 2

Figure 3. The SEM micrograph of a cleaved GaN/SiC sample with a stripe-like mesa structure formed by RIE in CCl2F2:Ar (12 sccm : 12 sccm) at 10 mTorr. The Ni mask, deposited by e-beam sputtering, is not removed.

Figure 3

Figure 4. The Rtot dependence of ln(R/r) for Ni contact on p-GaN.