Hostname: page-component-cd9895bd7-fscjk Total loading time: 0 Render date: 2024-12-26T08:03:38.220Z Has data issue: false hasContentIssue false

Direct Observation of PFIB-Induced Clustering in Precipitation-Strengthened Al Alloys by Atom Probe Tomography

Published online by Cambridge University Press:  24 January 2022

David Tweddle
Affiliation:
Department of Metallurgical & Materials Engineering, University of Alabama, Tuscaloosa, AL 35405, USA
Jonathan A. Johnson
Affiliation:
Department of Metallurgical & Materials Engineering, University of Alabama, Tuscaloosa, AL 35405, USA
M. Kapoor
Affiliation:
Novelis Global Research & Technology Center, 1950 Vaughn Road, Kennesaw, GA 30144, USA
Sean Mileski
Affiliation:
Novelis Global Research & Technology Center, 1950 Vaughn Road, Kennesaw, GA 30144, USA
John E. Carsley
Affiliation:
Novelis Global Research & Technology Center, 1950 Vaughn Road, Kennesaw, GA 30144, USA
Gregory B. Thompson*
Affiliation:
Department of Metallurgical & Materials Engineering, University of Alabama, Tuscaloosa, AL 35405, USA
*
*Corresponding author: Gregory B. Thompson, E-mail: gthompson@eng.ua.edu

Abstract

The effect of sample preparation on a pre-aged Al–Mg–Si–Cu alloy has been evaluated using atom probe tomography. Three methods of preparation were investigated: electropolishing (control), Ga+ focused ion beam (FIB) milling, and Xe+ plasma FIB (PFIB) milling. Ga+-based FIB preparation was shown to introduce significant amount of Ga contamination throughout the reconstructed sample (≈1.3 at%), while no Xe contamination was detected in the PFIB-prepared sample. Nevertheless, a significantly higher cluster density was observed in the Xe+ PFIB-prepared sample (≈25.0 × 1023 m−3) as compared to the traditionally produced electropolished sample (≈3.2 × 1023 m−3) and the Ga+ FIB sample (≈5.6 × 1023 m−3). Hence, the absence of the ion milling species does not necessarily mean an absence of specimen preparation defects. Specifically, the FIB and PFIB-prepared samples had more Si-rich clusters as compared to electropolished samples, which is indicative of vacancy stabilization via solute clustering.

Type
Materials Science Applications
Creative Commons
Creative Common License - CCCreative Common License - BY
This is an Open Access article, distributed under the terms of the Creative Commons Attribution licence (https://creativecommons.org/licenses/by/4.0/), which permits unrestricted re-use, distribution, and reproduction in any medium, provided the original work is properly cited.
Copyright
Copyright © The Author(s), 2022. Published by Cambridge University Press on behalf of the Microscopy Society of America

Introduction

Heat-treatable Al alloys, and other light metals such as Mg, are susceptible to room-temperature aging. As these alloy microstructures evolve, these changes detrimentally impact subsequent processing such as joining, forming, and even aging kinetics resulting in a “shelf-life” to the alloy. The clustering of solute atoms, which control these performance criteria, is strongly dependent on the vacancy super-saturation (Aruga et al., Reference Aruga, Kozuka, Takaki and Sato2015; Poznak et al., Reference Poznak, Marceau and Sanders2018). These solute clusters, particularly in the early stages of aging, are often difficult, if not impossible, to be resolved using transmission electron microscopy (TEM) because of their size and coherent structure within the matrix. In contrast to TEM, atom probe tomography (APT), a field ion microscopy method, can resolve as well as quantify the distribution characteristics of such clusters in these early stages. APT has equal sensitivity for all elements with an analytical sensitivity of approximately 5 atomic ppm and can reconstruct the spatial location of each atom with near-perfect lattice rectification (Marquis & Hyde, Reference Marquis and Hyde2010; Larson et al., Reference Larson, Prosa, Ulfig, Geiser, Kelly and Humphreys2013; Stephenson et al., Reference Stephenson, Moody, Gault and Ringer2013). Consequently, these attributes make this technique well suited to reveal the early stages of clustering in light metal alloys during aging at room and elevated temperatures (Buha et al., Reference Buha, Lumley, Crosky and Hono2007; Aruga et al., Reference Aruga, Kozuka, Takaki and Sato2015; Marceau, Reference Marceau2016; Buchanan et al., Reference Buchanan, Colas, Ribis, Lopez and Garnier2017; Hu et al., Reference Hu, Liu, Zhang and Sha2020; Lee et al., Reference Lee, Jung, Baik, Seidman, Kim, Lee and Euh2021).

APT requires an ultra-sharp needle-shaped specimen (r < 50 nm) to enhance the electric field at the tip required for field evaporation of the surface atoms. Historically, APT specimens were shaped using electropolishing which produces specimens that are essentially “damage-free.” In the past 20 years, the use of a Ga+ focused ion beam (FIB) has become ubiquitous for APT preparation as it enables site-specific preparation of APT samples (Larson et al., Reference Larson, Foord, Petford-long, Blamire, Cerezo and Smith1999). While inordinately beneficial to preparation, the Ga+ FIB does create unintended artifacts during sample preparation including amorphization of the surface (Miller et al., Reference Miller, Russell, Thompson, Alvis and Larson2007), creation of vacancies and other point defects from “knock-on” collisions within the alloy (Idrissi et al., Reference Idrissi, Turner, Mitsuhara, Wang, Hata, Coulombier, Raskin, Pardoen, Van Tendeloo and Schryvers2011), and embrittlement of the grain boundaries in Al alloys (Unocic et al., Reference Unocic, Mills and Daehn2010). The impact of such defects modifies precipitation transformation pathways and accelerates aging kinetics in Al alloys (Wang et al., Reference Wang, Jiang, Fan, Panindre, Frankel and Zhen2017).

Recent work by Lilensten & Gault (Reference Lilensten and Gault2020) on a commercial 6016 Al alloy has shown that cryogenic cooling during FIB lift-out and sharpening (performed at 82 K) reduces Ga+ diffusion to the grain boundaries. While this work focused on the impact of temperature during sample preparation with a particular emphasis on Ga+ grain boundary segregation, it did not specifically address the impact of milling created defects on solute clustering. Such knowledge is critical in elucidating the link between solute clustering and mechanical properties. Another potential strategy for light metals to mitigate ion milling damage during preparation is the use of the recently introduced plasma-based FIB (PFIB) (Halpin et al., Reference Halpin, Webster, Gardner, Moody, Bagot and MacLaren2019; Famelton et al., Reference Famelton, Hughes, Williams, Barbatti, Moody and Bagot2021). This microscope employs a Xe gas to create a plasma whereupon the ions are extracted for milling. Xe is believed to mitigate prior FIB risks because it is chemically inert (Halpin et al., Reference Halpin, Webster, Gardner, Moody, Bagot and MacLaren2019) and has decreased penetration depth/stopping distance for the same acceleration voltage, as shown by reducing up to 40% of the amorphous damage (in Si) as compared to Ga FIBs (Kelley et al., Reference Kelley, Song, Van Leer, Wall and Kwakman2013).

To date, there have been a limited number of studies that have specifically investigated the impact of point defects introduced during FIB-based sample preparation on the early stages of solute clustering behavior (Dumitraschkewitz et al., Reference Dumitraschkewitz, Gerstl, Uggowitzer, Löffler and Pogatscher2017; Famelton et al., Reference Famelton, Hughes, Williams, Barbatti, Moody and Bagot2021). As noted above, this is especially relevant for light metals where solute atoms are keenly sensitive to the disruptions in the lattice as they partition (Marceau, Reference Marceau2016). Recognizing the ever-increasing use of FIB milling methods to prepare APT needles, and the emerging PFIB options, this work investigates how such sample preparation, particularly the PFIB, alters the intrinsic nanostructure that ultimately influences the quantitative data that APT provides.

Methods

The Al–Mg–Si–Cu alloy, with a nominal bulk composition of Mg (0.7–1.0 wt%), Cu (0.6–0.9 wt%), Si (0.6–0.9 wt%), and remaining total minor elements (<1 wt%), was solution-treated followed by a low-temperature aging treatment at 100°C/4 h, denoted as pre-aging (PA). After PA, the case study alloy was immediately transferred to a freezer, to mitigate the impact of secondary natural aging (SNA) at room temperature (RT), and stored below −30°C till sample preparation. Additionally, a sample was electropolished following 30 days of SNA to deconvolute the impact of the sample preparation times on clustering behavior. Since electropolishing does not involve ion energy impact, but rather a gradual removal of material, these specimens are considered the control or intrinsic state of the case study alloy. The alloy in the PA condition was used as a case study for the following reasons: (1) This condition will have nucleated Mg-rich clusters. (2) There is enough solute dissolved in the matrix to capture the impact of the defects introduced during FIB sample preparation.

The electropolishing was performed using a conventional two-stage method (Yao & Zhong, Reference Yao and Zhong2005) with the sample cut into a rectangular geometry, denoted as a matchstick, and crimped into a Cu holding tube. In Stage 1, we utilized 10% perchloric acid in glacial acetic acid at 5 V DC until necking and separation of the matchstick occurred. In Stage 2, a mixture of 2% perchloric acid in butoxyethanol was used, again at 5 V DC, to ensure a sharp-needle-shaped specimen with a radius of <50 nm. After electropolishing, a minor contamination of Cu was observed on the tip surface (which is contributed to the electrolytic solution inadvertently contacting the copper tube holding the APT tip). Famelton et al. (Reference Famelton, Hughes, Williams, Barbatti, Moody and Bagot2021) also noted a similar electropolishing artifact. For both works, this surface area of copper contamination was excluded from the subsequent analysis. This preparation process took approximately 4 h to complete including sectioning of the rectangular “matchstick” that was then electropolished at one end into the APT tip. Ga+ FIB was performed using a Tescan Lyra FIB/SEM with trenching out the region of interest at 30 kV with 1–4 nA, while sharpening was performed at 30 kV between 30–300 pA. A low-kV clean-up step was performed in the final polish at 2 kV and 120 pA to reduce ion damage (Thompson et al., Reference Thompson, Gorman, Larson, van leer and Hong2006). The Xe+ PFIB was performed using a Thermo Fisher Scientific Helios G4 PFIB CXe dual-beam FIB/SEM with initial trenching and sharpening at 30 kV and 30–3000 pA, while final polishing was performed at 2 kV and 80 pA. Effort was made to ensure the milling currents and conditions used between the two FIB instruments at each stage were as equivalent as possible. The ion milling process, regardless of instrument, took between 4 and 6 h.

APT analysis was performed on a LEAP 5000 XS in voltage mode at 35 K, with a pulse fraction of 20%, a detection rate of 0.5%, and a pulse frequency of 200 kHz. Reconstructions were performed using IVAS 3.8.4, with pole indexing and spatial distribution maps used to optimize the reconstruction parameters (Breen et al., Reference Breen, Moody, Ceguerra, Gault, Araullo-Peters and Ringer2015). The cluster search was performed on a region of interest away from the poles using the maximum separation method, as described by Hyde et al. (Reference Hyde, Marquis, Wilford and Williams2011). To ensure consistency in the analysis of the different sample preparation methods, a value of 0.5 for the d max and a N min value of 17 with solute of Mg, Si, and Cu were used for each sample. In addition, the voltage range over which the data analysis was performed was between 3 kV and 5 kV. These values of d max and N min were selected by comparing the acquired data to a randomized dataset with the same solute concentration. Cluster searching on both datasets was then performed, with the selected values of d max and N min having the largest number of clearly discernible clusters compared to noise.

The number density of the clusters (NV) was calculated as follows:

(1)$$N_V = \displaystyle{{N\rho _{th}\eta } \over {N_{{\rm total}}}} , $$

where N is the number of clusters, ρ th is the theoretical density of the cluster (taken to be the same as the atomic density of Al), η is the detection efficiency of the LEAP 5000XS (80%), and N total is the total number of ions in the dataset (Jenkins et al., Reference Jenkins, Douglas, Almirall, Riddle, Bagot, Hyde, Odette and Moody2020). The error of the number density is given as NV divided by the square root of the total number of clusters.

Stopping and range of ions in matter (SRIM) modeling was performed using the SRIM 2013 software developed by Ziegler et al. (Reference Ziegler, Ziegler and Biersack2010). Xe and Ga ions were implanted perpendicularly into a pure Al target with a depth of 100 nm and a width of 100 nm. The total implanted ion count was 50,000 ions.

Results and Discussion

Figures 1a1c are representative APT reconstructions showing only the clusters identified, using the nearest neighbor search algorithm, in samples prepared using the three preparation methods: electropolishing (which served as the control), FIB, and PFIB. All three methods reveal qualitatively similar clustering. No Xe+ implantation in the PFIB sample was detected consistent with the absence of any peaks in the mass spectrum range of Xe+, Figure 1d. In contrast, the reconstruction of the Ga+ FIB sample reveals the presence of Ga, both in the mass spectrum, Figure 1e, and in the inset image in the same figure showing its concentration enrichment in the data volume. Here, the Ga accounted for ≈1.3 at% of the total collected ions. The absence of Xe+ could be explained by two things: (1) the lower penetration depth of Xe, as compared to Ga (Kelley et al., Reference Kelley, Song, Van Leer, Wall and Kwakman2013), and (2) Xe being a gas at standard conditions and would diffuse out of the tip and be lost to the atmosphere. The lack of Xe+ detected in the sample, unlike Ga+, could provide indications that this method of ion milling does not result in significant artifacts introduced into the nanostructure. In the recent work by Famelton et al. (Reference Famelton, Hughes, Williams, Barbatti, Moody and Bagot2021), where they used a PFIB to prepare APT tips from a 6xxx alloy, they noted Xe+ capture in their APT data volume sets, suggesting potential user-dependent variations in PFIB-prepared APT samples.

Fig. 1. Clusters detected in (a) a Xe+ PFIB sample dataset, (b) a Ga+ FIB sample dataset, and (c) an electropolished sample dataset. Extracts of the mass spectra from (d) a Xe+ PFIB sample dataset and (e) a Ga+ FIB sample dataset with a clear Ga+ peak and an inset image of the Ga concentration in the reconstruction visualized volume via density (where red indicates higher Ga concentration).

While the clusters qualitatively exist between each method, a detailed evaluation of their distribution characteristics reveals notable differences. Table 1 notes a significant modification in the number density of clusters. Specifically, Ga+ FIB- and Xe+ PFIB-prepared samples have approximately a doubling and nearly an order of magnitude increase in clusters for each method, respectively, as compared to the electropolished control sample. Interestingly, the cluster size is not significantly different among all the prepared samples, suggesting that the two observations from the control are not governed by kinetics. Recognizing that the number density could be influenced by differences in ambient temperature exposure from handling variations among the three preparation methods, an electropolished-prepared tip was studied from a pre-aged sample but allowed to naturally age for 30 days at ambient temperature (denoted as PA + NA/30 days). As can be seen in the tabulated results in Table 1, the number density slightly increased from 3.2 ± 0.4 × 1023 to 4.5 ± 0.8 × 1023 m−3 for this sample but is still lower than either the FIB or PFIB samples. This reinforces the deduction that the significant increase in cluster density is indeed a result of the specimen preparation method and not from potential (minor) handling differences between the preparation times among the three samples.

Table 1. Cluster Radius, Number Density, and the Percentage of Si-Rich of Clusters Detected in Samples Prepared via All Sample Preparation Methods.

To further confirm that the sample preparation method impacts cluster formation, the cluster compositions were examined based on their Mg:Si ratio. Figure 2 is the histograms of the Mg:Si ratio where a clear demarcation between the electropolished, Ga+ FIB, and the Xe+ PFIB exists. Specifically, the percentage of Si-rich clusters in the electropolished samples is 33%, Table 1, whereas in the FIB and PFIB samples, the Si-rich clusters are approximately 50 and 55%, respectively. Of the two ion milling methods, the clusters in Ga+ FIB did not reveal a clear separation based on solute enrichment, quantified via the Mg:Si ratio compared to either the electropolished sample or the PFIB sample. Collectively, the number density increases and the change in the cluster composition provide strong, quantitative evidence that these differences are driven by the sample preparation method, i.e., the clusters have nucleated during ion milling.

Fig. 2. Relative frequency histogram of the Mg:Si ratio of the clusters detected in the electropolished-, Ga+ FIB-, and Xe+ PFIB-prepared Al–Mg–Si samples.

The observations of a higher cluster number density and the nucleation of more Si-rich clusters can be explained by the clustering sequence after rapidly quenching an Al–Mg–Si alloy. When such an alloy is quenched from solution treatment temperatures, the Si atoms are the first to diffuse to the quenched-in vacancy clusters to stabilize them (Poznak et al., Reference Poznak, Marceau and Sanders2018) since Si has a positive binding energy and Mg has a negative binding energy to such vacancies (Wolverton, Reference Wolverton2007; Wang et al., Reference Wang, Jiang, Fan, Panindre, Frankel and Zhen2017). Therefore, the initial clusters that form at room temperature are Si-rich clusters, and over a period of few days of natural aging, Mg atoms will then segregate to the Si-vacancy stabilized clusters forming the observed Mg/Si co-clusters. Thus, the formation of Si-rich clusters is a distinct chemical signature of the newly formed clusters. The clear increase in Si-rich clusters in the PFIB sample and the balance of Si-rich and Mg-rich clusters in the FIB sample reveal that the ion milling has indeed facilitated an increase in the vacancy concentration that enabled the Si in solution to now cluster by the introduction of vacancies created during milling. Furthermore, coupling the increase in Si-rich clusters with the higher total cluster density in the PFIB sample as compared to the FIB sample provides further evidence that the Xe+ promoted a higher fraction of vacancy formation. Therefore, the number density and the chemical signature of these clusters (Si-rich versus Mg-rich) offer a direct means to measure how milling artificially evolved the nanostructure, even when the milling ions are not detected in the mass spectrum. This is further highlighted in the electropolished (PA + NA/30 days) sample in which the cluster characteristics are closer to the electropolished sample without any secondary natural aging. In the Famelton et al. (Reference Famelton, Hughes, Williams, Barbatti, Moody and Bagot2021) report, where PFIB preparation was used, an increase in clusters was noted but attributed to a larger sampling volume. Additionally, average cluster compositions were provided. While the study concludes that PFIB results in minimal sample preparation artifacts, the above results strongly indicate otherwise. These results do suggest a checkpoint in the interpretation of APT data from PFIB-prepared samples, particularly for the early stages of cluster formation.

To understand the relative impact of Ga+ and Xe+ impingement on vacancy formation, SRIM modeling was performed (Ziegler et al., Reference Ziegler, Ziegler and Biersack2010). The Xe+ and Ga+ were implanted perpendicular to a pure Al surface with the vacancy profiles in Al for the Xe and Ga implantation plotted in Figure 3. Although Ga implantation results in vacancy formation at greater depth, Xe-based implantation results in a much higher surface vacancy concentration at a depth of up to 30 nm at 30 kV. This results in a large concentration of Xe-induced vacancies, some of which diffuse out of the needle to the free surface and are annihilated (Dumitraschkewitz et al., Reference Dumitraschkewitz, Uggowitzer, Gerstl, Löffler and Pogatscher2019). Nonetheless, it is likely that a significant number of these vacancies will become stabilized by the dissolved solute Si atoms in the alloy forming the observed Si-rich clusters discussed above. This process of clustering is extremely fast and occurs within 15 s at 0°C to stabilize such vacancy clustering (Ozawa & Kimura, Reference Ozawa and Kimura1970). This finding is critical because it demonstrates that Xe+ PFIB-prepared samples can indeed generate artificially higher cluster number densities in Al alloys. Although 2 kV polishing was used to minimize the FIB and PFIB-related damage, SRIM modeling indicates that vacancies are still induced up to 5 nm into the surface. For the Ga+ FIB-prepared sample, the significant concentration of Ga found throughout the sample (≈1.3 at%) indicates severe implantation which likely contributed to amorphization of the surface (consistent with large amounts of Ga at the surface, see inset image in Fig. 1e) and that existing clusters being annihilated under implantation explains the modest increase in the cluster density as compared to the electropolished sample.

Fig. 3. SRIM calculated vacancy profiles for Ga and Xe implantation at 30 and 2 kV in Al.

Conclusion

This work reveals, quantitively, the substantial impact that ion milling can have on the solute clustering quantification in aluminum alloys using APT. Through a series of controlled experiments, the chemical signature of Si-rich clustering, as well as the increase in cluster density, provides supporting evidence that this ion milling creates new vacancies through implantation and knock-on events. Unlike Ga+ FIB milling, where the ion species is captured in the APT reconstruction providing direct chemical signature evidence of potential artifacts, the Xe+ PFIB ions were absent in its APT reconstruction. While this ion signature is not present, the PFIB milling has a higher deleterious artifact impact to the changes in the clustering nanostructure. Specifically, an increase in cluster density as compared to preparation where electropolishing or FIB milling is used results in the increase in vacancy density created by the Xe+. As Xe+ PFIB becomes an increasingly used as a tool in preparing Al alloys, these noted artifacts should be considered with any quantitative analysis and conclusion of the nanostructure, particularly with respect to the early stages of clustering.

Acknowledgments

The authors gratefully recognize Novelis Global Research & Technology Center for support of this research. The authors thank Dr. Debdutta Roy and Dr. Rajeev Kamat for contributing to insightful discussions. The Alabama Analytical Research Center, supported under the UA Office for Research and Economic Development, is also acknowledged.

References

Aruga, Y, Kozuka, M, Takaki, Y & Sato, T (2015). Formation and reversion of clusters during natural aging and subsequent artificial aging in an Al-Mg-Si alloy. Mater Sci Eng A 631, 8696.CrossRefGoogle Scholar
Breen, AJ, Moody, MP, Ceguerra, Av, Gault, B, Araullo-Peters, VJ & Ringer, SP (2015). Restoring the lattice of Si-based atom probe reconstructions for enhanced information on dopant positioning. Ultramicroscopy 159, 314323.CrossRefGoogle ScholarPubMed
Buchanan, K, Colas, K, Ribis, J, Lopez, A & Garnier, J (2017). Analysis of the metastable precipitates in peak-hardness aged Al-Mg-Si(-Cu) alloys with differing Si contents. Acta Mater 132, 209221.CrossRefGoogle Scholar
Buha, J, Lumley, RN, Crosky, AG & Hono, K (2007). Secondary precipitation in an Al-Mg-Si-Cu alloy. Acta Mater 55, 30153024.CrossRefGoogle Scholar
Dumitraschkewitz, P, Gerstl, SSA, Uggowitzer, PJ, Löffler, JF & Pogatscher, S (2017). Atom probe tomography study of As-quenched Al–Mg–Si alloys. Adv Eng Mater 19, 15.CrossRefGoogle Scholar
Dumitraschkewitz, P, Uggowitzer, PJ, Gerstl, SSA, Löffler, JF & Pogatscher, S (2019). Size-dependent diffusion controls natural aging in aluminium alloys. Nat Commun 10, 16.CrossRefGoogle ScholarPubMed
Famelton, JR, Hughes, GM, Williams, CA, Barbatti, C, Moody, MP & Bagot, PAJ (2021). Xenon plasma focussed ion beam preparation of an Al-6XXX alloy sample for atom probe tomography including analysis of an α-Al(Fe, Mn)Si dispersoid. Mater Charact 178, 112.CrossRefGoogle Scholar
Halpin, JE, Webster, RWH, Gardner, H, Moody, MP, Bagot, PAJ & MacLaren, DA (2019). An in-situ approach for preparing atom probe tomography specimens by xenon plasma-focussed ion beam. Ultramicroscopy 202, 121127.CrossRefGoogle ScholarPubMed
Hu, R, Liu, J, Zhang, Y & Sha, G (2020). Revealing solute clusters in coalescence by atom probe tomography analysis. Microsc Microanal 26, 10791087.CrossRefGoogle ScholarPubMed
Hyde, JM, Marquis, EA, Wilford, KB & Williams, TJ (2011). A sensitivity analysis of the maximum separation method for the characterisation of solute clusters. Ultramicroscopy 111, 440447.CrossRefGoogle ScholarPubMed
Idrissi, H, Turner, S, Mitsuhara, M, Wang, B, Hata, S, Coulombier, M, Raskin, J, Pardoen, T, Van Tendeloo, G & Schryvers, D (2011). Point defect clusters and dislocations in FIB irradiated nanocrystalline aluminium films: An electron tomography and aberration-corrected high-resolution ADF-STEM study. Microsc Microanal 17, 983990.CrossRefGoogle ScholarPubMed
Jenkins, BM, Douglas, JO, Almirall, N, Riddle, N, Bagot, PAJ, Hyde, JM, Odette, GR & Moody, MP (2020). The effect of composition variations on the response of steels subjected to high fluence neutron irradiation. Materialia 11, 111.CrossRefGoogle Scholar
Kelley, RD, Song, K, Van Leer, B, Wall, D & Kwakman, L (2013). Xe+ FIB milling and measurement of amorphous silicon damage. Microsc Microanal 19, 862863.CrossRefGoogle Scholar
Larson, DJ, Foord, DT, Petford-long, AK, Blamire, MG, Cerezo, A & Smith, GDW (1999). Field-ion specimen preparation using focused ion-beam milling. Ultramicroscopy 79(1–4), 287293.CrossRefGoogle Scholar
Larson, DJ, Prosa, TJ, Ulfig, RM, Geiser, BP, Kelly, TF & Humphreys, CJ (2013). Local Electrode Atom Probe Tomography a User's Guide. New York, Springer.Google Scholar
Lee, SH, Jung, JG, Baik, Si, Seidman, DN, Kim, MS, Lee, YK & Euh, K (2021). Precipitation strengthening in naturally aged Al–Zn–Mg–Cu alloy. Mater Sci Eng A 803, 18.CrossRefGoogle Scholar
Lilensten, L & Gault, B (2020). New approach for FIB-preparation of atom probe specimens for aluminum alloys. PLoS ONE 15, 19.CrossRefGoogle ScholarPubMed
Marceau, RKW (2016). Atomic scale analysis of light alloys using atom probe tomography. Mater Sci Technol 32, 209219.CrossRefGoogle Scholar
Marquis, EA & Hyde, JM (2010). Applications of atom-probe tomography to the characterisation of solute behaviours. Mater Sci Eng R Rep 69, 3762.CrossRefGoogle Scholar
Miller, MK, Russell, KF, Thompson, K, Alvis, R & Larson, DJ (2007). Review of atom probe FIB-based specimen preparation methods. Microsc Microanal 13, 428436.CrossRefGoogle ScholarPubMed
Ozawa, E & Kimura, H (1970). Excess vacancies and the nucleation of precipitates in aluminum-silicon alloys. Acta Metall 18, 9951004.CrossRefGoogle Scholar
Poznak, A, Marceau, RKW & Sanders, PG (2018). Composition dependent thermal stability and evolution of solute clusters in Al-Mg-Si analyzed using atom probe tomography. Mater Sci Eng A 721, 4760.CrossRefGoogle Scholar
Stephenson, LT, Moody, MP, Gault, B & Ringer, SP (2013). Nearest neighbour diagnostic statistics on the accuracy of APT solute cluster characterisation. Philos Mag 93, 975989.CrossRefGoogle Scholar
Thompson, K, Gorman, B, Larson, D, van leer, B & Hong, L (2006). Minimization of Ga induced FIB damage using low energy clean-up. Microsc Microanal 12(S02), 17361737.CrossRefGoogle Scholar
Unocic, KA, Mills, MJ & Daehn, GS (2010). Effect of gallium focused ion beam milling on preparation of aluminium thin foils. J Microsc 240, 227238.CrossRefGoogle ScholarPubMed
Wang, SS, Jiang, JT, Fan, GH, Panindre, AM, Frankel, GS & Zhen, L (2017). Accelerated precipitation and growth of phases in an Al-Zn-Mg-Cu alloy processed by surface abrasion. Acta Mater 131, 233245.CrossRefGoogle Scholar
Wolverton, C (2007). Solute-vacancy binding in aluminum. Acta Mater 55, 58675872.CrossRefGoogle Scholar
Yao, N & Zhong, LW (2005). Handbook of Microscopy for Nanotechnology. New York, Kluwer Academic Publishers.CrossRefGoogle Scholar
Ziegler, JF, Ziegler, MD & Biersack, JP (2010). SRIM—The stopping and range of ions in matter. Nucl Instrum Methods Phys Res B 268, 18181823.CrossRefGoogle Scholar
Figure 0

Fig. 1. Clusters detected in (a) a Xe+ PFIB sample dataset, (b) a Ga+ FIB sample dataset, and (c) an electropolished sample dataset. Extracts of the mass spectra from (d) a Xe+ PFIB sample dataset and (e) a Ga+ FIB sample dataset with a clear Ga+ peak and an inset image of the Ga concentration in the reconstruction visualized volume via density (where red indicates higher Ga concentration).

Figure 1

Table 1. Cluster Radius, Number Density, and the Percentage of Si-Rich of Clusters Detected in Samples Prepared via All Sample Preparation Methods.

Figure 2

Fig. 2. Relative frequency histogram of the Mg:Si ratio of the clusters detected in the electropolished-, Ga+ FIB-, and Xe+ PFIB-prepared Al–Mg–Si samples.

Figure 3

Fig. 3. SRIM calculated vacancy profiles for Ga and Xe implantation at 30 and 2 kV in Al.