Hostname: page-component-78c5997874-g7gxr Total loading time: 0 Render date: 2024-11-13T05:13:20.474Z Has data issue: false hasContentIssue false

GaN Homoepitaxy for Device Applications

Published online by Cambridge University Press:  13 June 2014

M. Kamp
Affiliation:
Dept. of Optoelectronics, University of Ulm, 89069 Ulm, GERMANY, Tel.: +49-731-5026050, Fax: +49-731-5026049, e-mail: markus.kamp@e-technik.uni-ulm.de
C. Kirchner
Affiliation:
Dept. of Optoelectronics, University of Ulm, 89069 Ulm, GERMANY, Tel.: +49-731-5026050, Fax: +49-731-5026049, e-mail: markus.kamp@e-technik.uni-ulm.de
V. Schwegler
Affiliation:
Dept. of Optoelectronics, University of Ulm, 89069 Ulm, GERMANY, Tel.: +49-731-5026050, Fax: +49-731-5026049, e-mail: markus.kamp@e-technik.uni-ulm.de
A. Pelzmann
Affiliation:
Dept. of Optoelectronics, University of Ulm, 89069 Ulm, GERMANY, Tel.: +49-731-5026050, Fax: +49-731-5026049, e-mail: markus.kamp@e-technik.uni-ulm.de
K.J. Ebeling
Affiliation:
Dept. of Optoelectronics, University of Ulm, 89069 Ulm, GERMANY, Tel.: +49-731-5026050, Fax: +49-731-5026049, e-mail: markus.kamp@e-technik.uni-ulm.de
M. Leszczynski
Affiliation:
High Pressure Research Center, Warsaw, POLAND
I. Grzegory
Affiliation:
High Pressure Research Center, Warsaw, POLAND
T. Suski
Affiliation:
High Pressure Research Center, Warsaw, POLAND
S. Porowski
Affiliation:
High Pressure Research Center, Warsaw, POLAND

Abstract

Epitaxial growth on GaN single bulk crystals sets new standards in GaN material quality. The outstanding properties provide new insights into fundamental material parameters (e.g. lattice constants, exciton binding energies, etc.) being not accessible by heteroepitaxial growth on sapphire or SiC. With MOVPE and MBE we realized unstrained GaN layers with dislocation densities about six orders of magnitude lower than in heteroepitaxy. Those layers revealed an exceptional optical quality as determined by a reduction of the photoluminescence linewidth from 5 to 0.1 meV and a reduced XRD rocking curve width from 400 to 20 arcsec.

Only recently, progress in surface preparation allowed morphologies of the layers suitable for device applications. We report on InGaN/GaN MQW structures as well as the first GaN pn- and InGaN/GaN double heterostructure LEDs on GaN single bulk crystals. Those LEDs are twice as bright as their counterparts grown on sapphire. In addition they reveal an improved high power characteristics, which is attributed to an enhanced crystal quality and an increased p-doping. Time resolved electroluminescence measurements proof that band/band recombination is the dominant emission mechanism for the InGaN/GaN LEDs.

Type
Research Article
Copyright
Copyright © 1999 Materials Research Society

Introduction

Due to its excellent optical and electrical properties, GaN attracts worldwide attention for devices and fundamental research. The wide direct bandgap, the high luminescence efficiency and the thermal, mechanical, and chemical robustness make group III-nitride semiconductors the superior material system for optoelectronic devices in the UV to visible range. Despite exceptional progress, group III-nitrides technology still suffers from mismatched heteroepitaxial growth. Mismatch in lattice constants and thermal expansion coefficients between substrate (mostly sapphire or SiC) and epitaxial layer inhibit perfect crystal formation, resulting in 109 to 1010 threading dislocations per cm2.

Homoepitaxial growth of GaN has proven its tremendous potential to achieve superior material quality resulting in extremely narrow photoluminescence (PL) linewidths [Reference Mayer, Pelzmann, Kamp, Ebeling, Teisseyre, Nowak, Leszczynski, Grzegory, Bockowski, Krukowski, Porowski and Karczewski1],[Reference Baranowski, Porowski, Scheffler and Zimmermann2] and a reduction of the dislocation densities by six orders of magnitude. These material qualities can only be attained using a substrate which is identical in crystal structure, lattice parameter and thermal expansion coefficient. Under those conditions, two-dimensional layer-by-layer growth can be obtained and the generation of dislocations can be inhibited. Additional process steps such as nitridation and nucleation layers, mandatory in heteroepitaxy of GaN, are no longer required, thus significantly simplifying the growth process. Besides the fundamental advantages of homoepitaxy, GaN substrates have a high thermal conductivity facilitating high power applications. Since they are electrically conductive, too, they provide additional freedom for the device design (e.g. vertical current transport) and simplify the device processing. Beside above mentioned advantages, GaN substrates are of particular interest for GaN-based blue laser, since simple facet cleaving [Reference Nakamura, Senoh, Nagahama, Iwasa, Yamada, Matsushita, Kiyoku, Sugimoto, Kozaki, Umemto, Sano and Chocho3] becomes feasible and the far field pattern will be improved due to the relative high index of refraction of the GaN substrates. These outstanding properties justify the enormous endeavor conducted at several laboratories on the growth of single crystal GaN substrates [Reference Karpinski, Jun and Porowski4],[Reference Detchprohm, Amano, Hiramatsu and Akasaki5],[Reference Sakai, Kurai, Nishino, Wada, Sato and Naoi6]. Even when the effort for those substrates is probably too high for mass products such as LEDs, it might be worth for high power laser applications.

Experimental

Substrate preparation

The GaN substrates have been grown in a high-temperature high-pressure process where the GaN is formed at N2 pressures up to 20 kbar and at temperatures up to 1600°C from atomic nitrogen dissolved in a Ga melt. At a growth rate of approximately 100 µm/h perpendicular to the c-plane, the wurtzite crystals are grown up to areas of some 100 mm2 at a thickness of about 200 µm. Undoped crystals used in this study reveal an flat (000−1) surface (i.e. N-polarity) and a rough (0001) surface (i.e. Ga-polarity), following E. Hellman’s convention on the orientation [Reference Hellman7]. The (000−1) surface can be mechano-chemically polished to achieve an atomically flat surface. The initial roughness of the (0001) side requires a polishing for device quality growth. Due to the chemically inertness of the (0001) surface this can only be achieved by mechanical polishing.

The crystal quality of the GaN substrates is excellent as indicated by x-ray rocking curve measurements [Reference Leszczynski, Teisseyre, Suski, Grzegory, Bockowski, Jun, Porowski, Pakula, Baranowski, Foxon and Cheng8]. Using Cu K α 1 radiation, linewidths of 20 arcsec are obtained for the (0002) reflex. The excellent structural properties are also pointed out by very low dislocation densities ranging from 103 − 105 cm−2. The optical quality however is poor, near-bandgap excitonic transitions are not visible, weak PL at 380 nm and at 530 nm is observed at room temperature (RT).

Epitaxial growth

The homoepitaxial growth of GaN is performed in a horizontal, RF heated, water cooled quartz MOVPE reactor (AIXTRON AIX 200 RF) operated at low pressures. Trimethylgallium (TMGa), Trimethylindium (TMIn), Trimethylaluminum (TMAl), ammonia (NH3), silan (SiH4) and bis-cyclopentadienylmagnesium (Cp2Mg) are used as precursors, hydrogen is used as carrier gas. The one side polished GaN substrates (approximately 8×6 mm2 in size) were heated to 1060°C under a steady flow of ammonia to avoid surface degradation. During growth, the flow rates of NH3 and TMGa were kept at 2.0 slm and 17 µmol/min, respectively. The Cp2Mg flow rate was 90 nmol/min for p-type doping. After growth, thermal annealing under nitrogen ambient at 750°C was performed for 5 min to obtain p-type conductivity.

Characterization

Photoluminescence measurements at RT and 4 K are performed using a HeCd laser (λ = 325 nm) with an excitation density of approx. 10 mW/mm2. X-ray diffraction (XRD) with CuKα 1 radiation is used to characterize the structural quality of the binary layers as well as the composition of the ternary ones. Hall measurements of the epitaxial layers are inhibited by the highly conductive GaN substrate.

Devices

LEDs are fabricated taking advantage of the vertical device structure. Ni/Au contacts (50/200 nm) are evaporated as p-contacts. Dicing is achieved by simple cleaving, since layer and substrate are identical in their crystal structure and orientation. Subsequently, the devices are mounted on a copper plate using silver glue as backside contact material (n-type). The LEDs are characterized by I-V measurements, their output power, and their electroluminescence spectra under cw- as well as ns-short-pulse-excitation.

Results and Discussion

Surface orientation and preparation

Both orientations (N-polarity (000−1) and Ga-polarity (0001)) of undoped single crystal substrates have been investigated in this study. Figure 1 compares the photoluminescence of GaN layers grown under identical conditions on GaN substrates of both orientations.

Fig 1.: Photoluminescence of epitaxial GaN layers (MBE) on (000−1)- and (0001)-oriented GaN substrates. Linewidth is as low as 0.5 meV for the (0001)-orientation.

At a PL linewidth of approx. 2 meV the material quality of the epitaxial layer grown on (000−1) oriented substrates compares favorably to heteroepitaxial growth. However, the properties of epitaxial films deposited on (0001) oriented substrates are clearly superior. Due to the outstanding material quality achieved on the (0001) oriented substrates (0.5 meV for the bound excitons in this MBE grown layer), this orientation has been used for the subsequently described work. The differences between both orientations can be traced back to the significantly different free surface energies of the orientations. From ab-initio calculations it is determined that the free surface energy of the (000−1) surface is significantly higher than the one of the (0001) surface [Reference Zywietz, Neugebauer, Scheffler, Northrup and Walle9]. From this point, the (0001) orientation provides a more stable surface with a lower probability of dopant incorporation [Reference Leszczynski and Meyer10].

For the following experiments the Ga-terminated side was mechanically polished to remove the initial roughness of the (0001) surface. This process, however, is known to create sub-surface damage which interferes with high quality epitaxial growth on such treated substrates. In conventional III-V technology, this damage is chemically removed, an approach not accessible for the nitrides, as there is no suitable etchant known. Therefore, chemically assisted ion beam etching (CAIBE), a dry etching technique where the physical and chemical components of the etching process can be controlled fairly independently, is used to remove residual sub-surface damage. For direct comparison one half of a sample is CAIBE treated, whereas the other part is left unetched. Therefore, the substrate surface is partially coated with photoresist, acting as an etch mask. Argon and chlorine gas are used as physical and chemical etching components, respectively. Within 10 minutes an etch depth of approx. 300 nm was achieved using an ion energy of 400 eV which is reduced to 100 eV towards the end to minimize the ion damage. Nevertheless, the process is supposed to create an ion damage up to a depth of 8 Å. Since the etch rate depends only weakly on the chlorine flux, the process is regarded to be dominated by the physical component, i.e. sputtering. Figure 2a shows a SEM micrograph of a homoepitaxial GaN layer grown on a substrate which has been treated as described above.

Fig 2.: SEM image (2a), corresponding cathodoluminescence (CL) intensities (2b) and local CL spectra (2c) obtained from an epitaxial GaN layer grown on partially CAIBE treated (0001)-oriented GaN substrates. CL by F. Bertram, T. Riemann, and J. Christen (Univ. Magdeburg).

The micrograph depicts the surface of a MOVPE grown GaN film just at the borderline between the etched and overgrown part (upper part) and the overgrown part which was not previously etched (lower part). The CAIBE-etched part of the sample reveals a significantly improved surface topology with almost no visible scratches, trenches, or holes. Figure 2b shows the corresponding CL intensity distribution of the same region of the sample. On the etched part, the intensity variation is almost negligible. In contrast, the area being not etched yields only weak CL signals (1000 times less in intensity) which also fluctuate locally. The comparison of the local CL spectra reveals large differences. The measured linewidth of the spectrum taken from the etched region (fig. 2a, area A) is ten times narrower than that of the non-etched region (fig. 2a, area B). However, the narrow CL spectra obtained from area A are still clearly resolution limited by the employed setup. The following mechanism is proposed to be responsible for the observations [Reference Schauler, Eberhard, Kirchner, Schwegler, Pelzmann, Kamp, Ebeling, Bertram, Riemann, Christen, Leszczynski, Grzegory, Suski and Porowski11]. After mechanical polishing, the bulk GaN substrates reveal a smooth and mirror-like surface, however, sub-surface damage is induced by the polishing. By heating the substrates to growth temperature under ammonia during the MOVPE process, the damage becomes obvious revealing the observed trenches and scratches in the surface (fig. 2a, lower part). This experimental finding can be understood by dissociation and subsequent desorption of the damaged GaN. Eventually, during the heat up phase of the MOVPE growth, the substrate temperature of about 1100°C becomes high enough to achieve chemical etching (dissociation) under NH3 even of non-deteriorated GaN layers [Reference Makarov and Karpov12]. Whenever CAIBE is applied before annealing, the originally mirrorlike surface morphology is kept mirrorlike during the mostly physical etching process and thereby transferred into the undisturbed part of the substrate. However, ion-beam induced damage is created by the CAIBE process. This damage, nevertheless, is distributed homogeneously over the sample surface. During annealing in the MOVPE system this damage will dissociate revealing an almost perfect and smooth surface. Excess metallic Ga left on the surface is desorpt due to the exceptional high growth temperature of the group III-nitrides.

The necessity of the CAIBE treatment for devices based on single crystal substrates can best be seen in Fig. 3 showing evaporated Ni/Au metal contacts on a GaN pn-junction LED in an area without (Fig. 3a) and with prior CAIBE treatment (Fig 3b). The region of the device which was not CAIBE-treated reveals deep trenches as described earlier. Since the depths of the trenches is above the typical thickness of the p-GaN layer any metallization covering the sidewalls of the trenches will short circuit the pn-junction of the device.

Fig. 3: SEM micrograph of the surface of a homoepitaxial GaN pn-junction LED with evaporated Ni/Au metal contacts, without (3a) and with (3b) CAIBE treatment prior to growth (different areas of the same sample).

Binary and ternary layer properties

Homoepitaxial GaN layers with outstanding properties have been achieved using above described CAIBE technique (Fig. 4). PL at 4.2 K reveals free excitons A, B, C as well as excited states of those excitons, where the identification is verified by reflectance measurements included in the figure. The linewidth of the bound excitons (3.464 – 3.474 eV) is as low as 0.1 meV.

Fig. 4: High resolution photoluminescence (log. scale) and reflectance (lin. scale) of a 2 µm epitaxial GaN layer grown on CAIBE treated (0001)-oriented GaN substrates. Measurements by K. Kornitzer, K. Thonke, and R. Sauer (Univ. Ulm, Dept. of Semiconductor Physics).

The structural quality of the homoepitaxial GaN layers is extremely high as indicated by the narrow linewidth of approx. 20 arcsec ((0002) reflex), revealing the low dislocation density and the negligible mosaicity of the GaN layers grown on single crystal GaN substrates. A minor lattice mismatch of approx. a/a 10−4 between layer and substrate is due to the high carrier concentration of the substrates [Reference Leszczynski, Teisseyre, Suski, Grzegory, Bockowski, Jun, Porowski, Pakula, Baranowski, Foxon and Cheng8]. The outstanding xray data confirm that homoepitaxial growth conserves or even improves the excellent structural quality and low dislocation density of the GaN substrates, as expected.

Ternary III-N compounds have been investigated as building blocks for double-heterostructure- (DH) and MQW-LEDs. The PL of 50 nm thick InGaN layers is shown in Fig 5. For comparison the PL of a heteroepitaxially layer grown under identical conditions (but employing a nucleation layer) is included. The observed shift in the emission wavelength can be understood by a different surface temperature between the highly heat conductive and partially absorbing GaN substrate and the sapphire. This causes a higher surface temperature for the GaN substrates at a nominally identical susceptor temperature, leading to a reduced In incorporation and the observed slightly lower emission wavelength. Fig 6. reveals a analogously comparison for InGaN/GaN (3nm/3nm) multiple quantum well structures.

Fig. 5: Room temperature photoluminescence of approx. 50 nm InGaN layers grown on GaN- and sapphire-substrates, respectively.

Fig. 6: Photoluminescence of InGaN/GaN (3nm/3nm) multiple quantum well structures grown on GaN- and sapphire-substrates, respectively (20 K).

Light emitting diodes

Initial LED structures have been homotype pn-junction LEDs. Only the regions of the device which underwent a CAIBE treatment yield functional devices, as becomes obvious from Fig. 3. The EL of those devices is depicted in Fig. 7 for various current densities. The LEDs show an intense, single peak emission at about 420 nm wavelength with a linewidth of 60 nm for low currents. UV emission is not observed even under the highest current densities. It is remarkable that the emission wavelength is constant at approx. 425 nm up to current densities of 3000 kA/cm2. As was initially pointed out by S.Nakamura et al. for GaN pn-junction LEDs this is a clear indicative of the high quality of the p-type material obtainable by homoepitaxial growth [Reference Nakamura, Mukai and Senoh13]. With increasing free hole concentration, the PL transition at 425 nm is found to increase in intensity [Reference Kaufmann, Kunzer, Maier, Obloh, Ramakrishnan, Santic and Schlotter14],[Reference Haffouz, Beaumont, Leroux, Laugt, Lorenzini, Gibart and Hubert-Pfalzgraf15]. Only a very high density of those recombination centers can guarantee an emission at 425 nm in EL even under high current densities. Once the injected carriers outnumber these recombination centers the surplus carriers recombine under emission of UV light at about 380 nm [Reference Calle, Monroy, Sánchez, Muñoz, Beaumont, Haffouz, Leroux and Gibart16]. The EL obtained from heteroepitaxial LEDs grown on sapphire under identical conditions is also included for comparison (dashed line). The heteroepitaxial devices reveal a clear shift towards shorter wavelengths which is attributed to an inferior quality of the p-material at the pn-junction. Furthermore, the homoepitaxial LED is approx. twice as bright as their counterpart on sapphire.

Fig. 7: Electroluminescence (EL) of a GaN homojunction pn-LED grown on GaN substrate. Emission spectra at various current densities. At a given current density, the homoepitaxial devices are twice as bright as comparable LEDs grown on sapphire (dashed line).

In addition to above homojunction LEDs, first InGaN/GaN DH-LEDs have been fabricated using single bulk crystal substrates. The EL of those devices is depicted in Fig. 8. Even at low current densities of 6 A/cm2 decent EL is observed revealing a significant lower density of non-radiative recombination centers than in their on-sapphire-grown counterparts. Time resolved EL is measured to reveal the recombination mechanisms (Fig. 9) [Reference Schwegler, Kirchner, Kamp, Ebeling, Leszczynski, Grzegory and Porowski17]. A single exponential decay with a time constant as low as 1 ns clearly identifies band/band recombination to be the dominant emission mechanism, since defect- as well as DAP-related electroluminescence transitions, as localized states, reveal a two order of magnitudes longer decay time (about 100 ns) [Reference Choa, Fan, Liu, Sipior, Rao, Carter and Chen18].

Fig. 8: Electroluminescence (EL) of a InGaN/GaN DH-LED grown on GaN substrate. Excellent EL is achieved at low current densities, revealing a low density of non-radiative defects.

Fig. 9: Time resolved electroluminescence (EL) of a InGaN/GaN DH-LED grown on GaN substrate. Depicted is the EL after short-pulse-excitation at 50 V for 10 ns (pulse being also depicted). Exponential decay time is as short as 1 ns indicating band/band recombination. The pulse-signal delay of 35 ns is caused by the experimental setup.

The current through the LED as depicted in Fig. 10 is obviously limited by the series resistance (i.e. contact and sheet resistances) of the devices, which can be deduced to about 1 kΩ from the currents at high voltages (UD larger than a few (nkBT)/q). The voltage drop at the series resistance is most likely caused by the imperfect housing of the LEDs, since the devices have just been glued to a metal base using silver glue. The current then is then passed through the 200 – 300 µm thick substrate of the vertical device. Further improvements are expected using a more elaborated contact and housing technology.

Fig. 10: Current/voltage characteristics of a GaN InGaN/GaN DH-LED. The curve reveals a good breakdown behavior and turn-on-voltage but still a rather high series resistance. The later is probably originated by contributions from the silver glue (n-contact metal) and the 200 − 300 µm thick n-layer (i.e. mostly the substrate).

Summary

After introduction of a CAIBE dry-etching step GaN layers with outstanding optical qualities and excellent morphologies have been achieved on bulk GaN single crystal substrates. Thick InGaN layers as well as InGaN/GaN MQWs are clearly superior to their counterparts grown on sapphire. Homoepitaxial GaN LEDs reveal single-peak blue emission at 420 nm, with a linewidth of 60 nm. The excellent quality of the homoepitaxial LEDs grown on GaN substrates is revealed by a comparison with heteroepitaxially LEDs on sapphire. The homoepitaxial devices are twice as bright as the LEDs grown on sapphire. This and the wavelength shift of the LED on sapphire are indications for a higher hole concentration of the homoepitaxial device. First InGaN/GaN DH-LEDs have been fabricated and reveal excellent electroluminescence at 455 nm even at low current densities, indicating a low density of non-radiative defects. Time resolved EL measurements performed on those devices clearly evince band/band recombination to be the dominant mechanism in those devices.

Acknowledgments

Several researchers severely contributed to this work, including M. Schauler, F. Eberhard, S. Menzel, and P. Unger from Dept. of Optoelectronics, F. Bertram, T. Riemann, and J. Christen from Univ. Magdeburg (CL measurements), K. Kornitzer, K. Thonke, and R. Sauer from Univ. Ulm, Dept. of Semiconductor Physics (high resolution PL measurements and reflectance). The authors gratefully acknowledge their valuable contributions as well as financial support by the German Federal Ministry of Education, Science, Research and Technology (BMBF) under contract no. 01 BM 419 / 9 and the Volkswagen Foundation.

Footnotes

MRS Internet J. Nitride Semicond. Res. 4S1, G10.2(1999)

References

Mayer, M., Pelzmann, A., Kamp, M., Ebeling, K.J., Teisseyre, H., Nowak, G., Leszczynski, M., Grzegory, I., Bockowski, M., Krukowski, S., Porowski, S., Karczewski, G., Jpn. J. Appl. Phys. Part 2, Vol. 36, L1634-L1636 (1997).Google Scholar
Baranowski, J., Porowski, S., Proc. 23rd Int. Conf. on the Physics of Semiconductors, Berlin 1996, edited by Scheffler, M. and Zimmermann, R. (World Scientific, Singapore 1996) vol. 3, (1996).Google Scholar
Nakamura, S., Senoh, M., Nagahama, S., Iwasa, N., Yamada, T., Matsushita, T., Kiyoku, H., Sugimoto, Y., Kozaki, T., Umemto, H., Sano, M., Chocho, K., Appl. Phys. Lett. 73, 832 (1998).Google Scholar
Karpinski, J., Jun, J. and Porowski, S.: J. Crystal Growth 66, 1-10 (1984).Google Scholar
Detchprohm, T., Amano, H., Hiramatsu, K. and Akasaki, I.: J. Crystal Growth 128, 384-390 (1993).Google Scholar
Sakai, S., Kurai, S., Nishino, K., Wada, K., Sato, H. and Naoi, Y.: Mat. Res. Soc. Symp. Proc. 449, 15-22 (1997).CrossRefGoogle Scholar
Hellman, E., MRS Internet J. Nitride Semicond. Res. 3, 11 (1998).Google Scholar
Leszczynski, M., Teisseyre, H., Suski, T., Grzegory, I., Bockowski, M., Jun, J., Porowski, S., Pakula, K., Baranowski, J.M., Foxon, C.T., Cheng, T.S., Appl. Phys. Lett. 69 (1), 73-75 (1996).Google Scholar
Zywietz, T., Neugebauer, J., Scheffler, M.,Northrup, J., Walle, Chris G. Van de, MRS Internet J. Nitride Semicond. Res. 3, 26(1998).Google Scholar
Leszczynski, M., Meyer, B.K., unpublished.Google Scholar
Schauler, M., Eberhard, F., Kirchner, C., Schwegler, V., Pelzmann, A., Kamp, M. Ebeling, K.J., Bertram, F., Riemann, T., Christen, J., Leszczynski, M., Grzegory, I., Suski, T., Porowski, S., accepted for Appl. Phys. Lett.Google Scholar
Makarov, Yu., Karpov, Yu., private communication.Google Scholar
Nakamura, S., Mukai, T. and Senoh, M.: Jpn. J. Appl. Phys. 30 No. 12A, L1998-L2001 (1991).Google Scholar
Kaufmann, U., Kunzer, M., Maier, M., Obloh, H., Ramakrishnan, A., Santic, B., Schlotter, P., Appl. Phys. Lett. 72 (11), 1326-1328 (1998).CrossRefGoogle Scholar
Haffouz, S., Beaumont, B., Leroux, M., Laugt, M., Lorenzini, P., Gibart, P., Hubert-Pfalzgraf, L.G., MRS Internet J. Nitride Semicond. Res. 2, 37 (1997).CrossRefGoogle Scholar
Calle, F., Monroy, E., Sánchez, F.J., Muñoz, E., Beaumont, B., Haffouz, S., Leroux, M., Gibart, P., MRS Internet J. Nitride Semicond. Res. 3, 24 (1998).Google Scholar
Schwegler, V., Kirchner, C., Kamp, M. Ebeling, K.J., Leszczynski, M., Grzegory, I., Porowski, S., submitted to Appl. Phys. Lett.Google Scholar
Choa, F.S., Fan, J.Y., Liu, P.L., Sipior, J., Rao, G., Carter, G.M., Chen, Y.J., Appl. Phys. Lett. 69 (24), 3668-3670 (1996).Google Scholar
Figure 0

Fig 1.: Photoluminescence of epitaxial GaN layers (MBE) on (000−1)- and (0001)-oriented GaN substrates. Linewidth is as low as 0.5 meV for the (0001)-orientation.

Figure 1

Fig 2.: SEM image (2a), corresponding cathodoluminescence (CL) intensities (2b) and local CL spectra (2c) obtained from an epitaxial GaN layer grown on partially CAIBE treated (0001)-oriented GaN substrates. CL by F. Bertram, T. Riemann, and J. Christen (Univ. Magdeburg).

Figure 2

Fig. 3: SEM micrograph of the surface of a homoepitaxial GaN pn-junction LED with evaporated Ni/Au metal contacts, without (3a) and with (3b) CAIBE treatment prior to growth (different areas of the same sample).

Figure 3

Fig. 4: High resolution photoluminescence (log. scale) and reflectance (lin. scale) of a 2 µm epitaxial GaN layer grown on CAIBE treated (0001)-oriented GaN substrates. Measurements by K. Kornitzer, K. Thonke, and R. Sauer (Univ. Ulm, Dept. of Semiconductor Physics).

Figure 4

Fig. 5: Room temperature photoluminescence of approx. 50 nm InGaN layers grown on GaN- and sapphire-substrates, respectively.

Figure 5

Fig. 6: Photoluminescence of InGaN/GaN (3nm/3nm) multiple quantum well structures grown on GaN- and sapphire-substrates, respectively (20 K).

Figure 6

Fig. 7: Electroluminescence (EL) of a GaN homojunction pn-LED grown on GaN substrate. Emission spectra at various current densities. At a given current density, the homoepitaxial devices are twice as bright as comparable LEDs grown on sapphire (dashed line).

Figure 7

Fig. 8: Electroluminescence (EL) of a InGaN/GaN DH-LED grown on GaN substrate. Excellent EL is achieved at low current densities, revealing a low density of non-radiative defects.

Figure 8

Fig. 9: Time resolved electroluminescence (EL) of a InGaN/GaN DH-LED grown on GaN substrate. Depicted is the EL after short-pulse-excitation at 50 V for 10 ns (pulse being also depicted). Exponential decay time is as short as 1 ns indicating band/band recombination. The pulse-signal delay of 35 ns is caused by the experimental setup.

Figure 9

Fig. 10: Current/voltage characteristics of a GaN InGaN/GaN DH-LED. The curve reveals a good breakdown behavior and turn-on-voltage but still a rather high series resistance. The later is probably originated by contributions from the silver glue (n-contact metal) and the 200 − 300 µm thick n-layer (i.e. mostly the substrate).