Vapour phase hydration studies of a blended Oxide / Magnox simulant high level waste glass were undertaken at 200°C, over a period of 5 – 25 days. The alteration of this simulant waste glass is characterised by a short incubation time of less than 5 days, leading to the formation of an alteration layer several microns thick. Following the incubation period, the alteration proceeds at a constant rate of 0.15(1)μmd−1. The distribution of key glass matrix (Si, Na) and waste (Cs, Zr, Nd, Mo) elements was found to vary significantly across the alteration layer. Vapour phase hydration leads to formation of surface alteration products, identified as smectite, zirconium silicate and alkaline-earth molybdate phases.