NiIn as an Ohmic Contact to P-GaN

Published online by Cambridge University Press:  13 June 2014

D. B. Ingerly
Affiliation:
Department of Materials Science and Engineering, University of Wisconsin, Madison, Wisconsin 53706-1595
Y. A. Chang
Affiliation:
Department of Materials Science and Engineering, University of Wisconsin, Madison, Wisconsin 53706-1595
Y. Chen
Affiliation:
Hewlett-Packard Company, 3500 Deer Creek Road, Palo Alto, California 94304-1392

Abstract

Based on the criteria for the solid state exchange reaction with p-GaN, we have investigated the intermetallic compound NiIn as a possible ohmic contact. The contacts were fabricated by depositing NiIn on p-GaN films (p ∼ 2 × 1017 cm−3) using RF sputtering from a compound target. The as-deposited, NiIn contacts were found to be rectifying and using I-V characterization a Schottky barrier height of 0.82 eV was measured. Rapid thermal annealing of the contacts was shown to significantly decrease their resistance, with contacts annealed at 800 °C for 1 min yielding the lowest resistance. When annealed at 800 °C for 1 min NiIn contacts exhibited a specific contact resistance of 8-9 × 10−3 Ω cm2 as measured by the circular transmission line model. To allow a more universal comparison the more traditional Ni/Au contacts, processed under the same conditions, were used as a standard. Their measured specific contact resistance (ρc = 1.2 − 2.1 × 10−2 Ωcm2) was significantly higher than that of the NiIn contacts. Demonstrating that NiIn has promise as an ohmic contact to p-GaN and should be studied in greater detail.

Type
Research Article
Copyright
Copyright © 1999 Materials Research Society

Introduction

It has long been realized that the III-V nitrides have tremendous potential for optoelectronic devices operating in the blue and UV wavelengths as well as for use in high power-high temperature semiconductor devices. The III-V nitrides form a continuous alloy system whose direct band gap ranges from 6.2 eV (AlN) to 3.4 eV (GaN) to 1.9 eV (InN) at room temperature.Reference Morkoc, Strite, Gao, Lin, Sverdlov and Burns 1 This potentially allows the fabrication of high efficiency optical devices, such as Light Emitting Diodes (LEDs), which can operate from orange to the UV region. The extension into the green and blue wavelengths completes the visible spectrum allowing semiconductor technology to be used for applications such as large full color displays and traffic lights.Reference Morkoc and Mohammad 2 , Reference Pearton and Kuo 3

Early research into the nitrides outlined several problem areas, which hindered efforts to produce devices based on III-V nitride technology. Particularly the lack of p-GaN made the fabrication of efficient optical devices based on p-n junctions impossible, though some LEDs based on metal-insulator-semiconductors were fabricated.Reference Morkoc, Strite, Gao, Lin, Sverdlov and Burns 1 , Reference Pearton and Kuo 3 Only recently due to advances in p-type doping has GaN started to realize its potential and there are now nitride based devices available. However, the metal contact to p-GaN is an important concern since high contact resistance will substantially reduce the performance of GaN based devices. In fact, the high resistance of the metal/p-GaN contact is one of the most significant issues limiting laser diode performance.

Most of the current work on finding low resistance metallizations to p-GaN has focused on high work function elemental metals deposited in multilayer structures.Reference Mori, Kozawa, Ohwaki, Taga, Nagai, Yamasaki, Asami, Shibata and Koike 4 Reference Soon, Kim, Park, Um, Han, Kim, Jang and Park 11 This strategy is based on the Schottky model, which predicts that higher work function metals will result in lower Schottky barriers to p-type semiconductors. The limited experimental evidence available on metal/p-GaN contacts suggests that the Schottky model is at least partially applicable.Reference Mori, Kozawa, Ohwaki, Taga, Nagai, Yamasaki, Asami, Shibata and Koike 4 Of the several contact schemes to p-GaN that have been studied Au/Ni contacts have received the most attention. Despite being used in devices, the Au/Ni contacts typically exhibit a specific contact resistance (ρc) in the range of 10−3 and 10−2 Ω cm2 rangeReference Kim, Yoo and Kim 7 , Reference King, Zhang, Ramer, Hersee and Lester 8 , Reference Nakamura 12 and show poor thermal stability.Reference Venugopalan, Mohney, Luther, DeLucca, Wolter, Redwing and Bulman 13 However, it is known that the specific contact resistance of p-GaN depends on many factors such as the quality of the bulk substrate and its surface preparation and processing conditions. Accordingly, it is difficult to judge the absolute resistance values reported.

In an attempt to find new metallizations that can be used to form ohmic contacts to p-GaN the solid-state exchange reaction was utilized. This reaction has been shown to be a systematic approach for tailoring metal/semiconductor contact properties.Reference Lin, Chang, Pan, Huang and Kuech 14 Reference Chen 17 The complete thermodynamic and kinetic model for the exchange mechanism has been comprehensively set forth by Swenson et al.Reference Swenson, Jan and Chang 18 Based on the exchange mechanism criteria, the intermetallic compound NiIn was selected as possible ohmic contact to p-GaN.

The thermodynamically stable phase of NiIn (50:50 at % ratio) has a CoSn (B35) crystal structure, however, the metastable B2 phase often forms and is the structure of the NiIn films used in this study. This B2 phase is thermodynamically stable at high temperature in Ni-In alloys that have 51 to 58 % In.Reference Okamoto and Massalski 19

Experimental Procedure

The GaN substrates used in this study are 1.2 μm thin films of single crystal GaN grown by metalorganic vapor phase epitaxy (MOVPE) on sapphire (0001). The GaN epilayer is Mg doped and was annealed to activate the dopants. A p-type carrier concentration of 2 × 1017 cm−3 with a mobility of 8 cm/V s was measured by Hall probe at room temperature. Prior to lithography, the substrates were ultrasonically degreased with Acetone and Methanol for 10 min each. These degreased substrates were then etched in HCl:H2O (1:2) for 4 min and then rinsed in flowing H2O for 10 min.

Using standard photolithography techniques the substrates were patterned with a circular transmission line model (TLM) pattern similar to the one detailed by Marlow.Reference Marlow and Das 20 Schottky barrier heights were measured by Current-Voltage (I-V) characteristics using the 140 μm diameter pad as the diode and the large area metallization as the ohmic contact. The specific contact resistance (ρc) measurements were conducted at 5 volts using the circular TLM pattern which consists of 7 different contact pads with gap spacing ranging from 4 to 25 µm. Once patterned, the substrates were then placed in a HCl:H2O (1:4) solution for 20 seconds, blown dry with Nitrogen gas and immediately loaded into a vacuum chamber with the background pressure less than 2 × 10−7 torr.

The NiIn (50:50 at % ratio) was deposited by sputtering from a compound target to a nominal 80 nm thickness. The annealed NiIn films were found by X-ray diffraction to be in the metastable B2 crystal structure when deposited by RF sputtering under the conditions used. As a control standard, Ni/Au contacts were also fabricated. These films were deposited by e-beam evaporation, with Ni and Au film thickness of 20 and 100 nm, respectively.

After deposition, the photoresist was lifted off in an acetone bath leaving the patterned metal on the wafers. Following liftoff, the contacts were annealed in an AG Associated MiniPulse rapid thermal annealing (RTA) system with flowing high purity Nitrogen gas. The electrical properties of the contacts were measured with a Keithley Model 236 electrometer employed as a current source and voltage meter.

Electrical Results

As discussed in the introduction, the intermetallic compound NiIn has been selected for study as an ohmic contact to p-GaN. However, it is difficult to compare the specific contact resistance for different metallizations reported by different researchers due to the wide variability in p-GaN substrates because these substrate differences can play an important role in the measured properties of the contacts. Therefore, in order to allow a more universal comparison of the NiIn metallization evaluated in this study we have used Ni/Au contacts as a standard.

All of the as-deposited contacts exhibited highly rectifying behavior; and it was decided that the Schottky barrier height is a more appropriate measure of these contacts’ electrical behavior than the ρc at a given voltage. By evaluating the I-V behavior at small voltages the Schottky barrier and ideality factor can be determined by fitting the data to the following equation:

(1)

where A* is the Richardson constant, S is the diode area, T is the temperature, q is the electron charge, φb is the Schottky barrier height, k is the Boltzman constant, V is the applied voltage and n is the ideality factor.Reference Schroder 21 Schottky barrier heights determined for the contacts in the as-deposited state are listed in Table 1. To the best of our knowledge, a value for NiIn on p-GaN has not been previously reported. However, the 0.77 eV value of the Schottky barrier height of Ni/p-GaN determined in this study is significantly higher than the 0.5 eV value reported by Mori, et al.Reference Mori, Kozawa, Ohwaki, Taga, Nagai, Yamasaki, Asami, Shibata and Koike 4 While the reason for such a discrepancy is not known, Ishikawa, et alReference Ishikawa, Kobayashi, Koide, Yamasaki, Nagai, Umezaki, Koike and Murakami 22 reported about the difficulty in measuring the barrier height of metals on p-GaN. Additionally the ideality factors for all of the contacts measured were significantly greater than 1; showing that the carrier transport mechanism is not entirely due to thermionic emission and suggesting that the interface is not uniform.Reference Tung and Vac 23 For the Schottky barrier measurement an ohmic contact is required in addition to the Schottky diode. In this study, the ohmic contact was approximated using a large area contact of the same metallization and while this contact is many times larger than the diode, it is not a true ohmic contact. Given the difficulties of measuring the barrier height of metals on p-GaN and the large ideality factors, the absolute value of barrier heights reported in this study should be interpreted accordingly.

Table 1. Ideality factors and Schottky barrier height for as-deposited contacts

Metallization Ideality Factor (n) Schottky Barrier Height
NiIn 1.22 0.82 eV
Ni/Au 1.16 0.77 eV

With increased annealing temperature the resistance of the NiIn/p-GaN contacts decreased. The lowest contact resistance occurs after annealing at 800 °C for 1 min, contacts subjected to a higher annealing temperature, 850 °C for 1 min or increased annealing time, 800 °C for 5 min showed a higher resistance than the samples annealed at 800 °C for 1 min. Table 2 gives the specific contact resistance on NiIn/p-GaN contacts at three different annealing conditions. One possibility for the increased resistances at more severe annealing conditions is oxidation of the NiIn layer. Scanning Auger Microscopy showed that significant oxidation occurred from the surface into over half of the NiIn film for contacts annealed at 800 °C for 1 min. It is possible that once a significant level of oxidation is reached at the metal/semiconductor interface the contact resistance will increase.

Table 2. Specific Contact Resistance for NiIn contacts

Annealing Conditions Specific Contact Resistance
750 °C for 1 min 6.2 × 10−2 Ωcm2
800 °C for 1 min 9.5 × 10−3 Ωcm2
800 °C for 5 min 7.4 × 10−2 Ωcm2

Due to the wide variability in p-GaN films and the direct role the films have in the measured specific contact resistance we have used Ni/Au contacts to p-GaN as a standard. Table 3 shows a comparison of NiIn contacts annealed at 800 °C for 1 min to Ni/Au annealed at 750 °C for 1 min. These contacts were subject to the same processing conditions and the annealing conditions used represent the optimum conditions found in this study for the two different metallizations. For both p-GaN substrates used, the NiIn contacts had a lower measured specific contact resistance than the Ni/Au contacts. Figures 1(a) and 1(b) show the I-V behavior of the annealed NiIn and Ni/Au contacts, respectively. These curves were measured on back-to-back 140 μm in diameter contacts. Figures 1(a) and 1(b) clearly show that these contacts do not exhibit true ohmic behavior.

Table 3. A comparison of specific contact resistance NiIn Vs. Ni/Au

Substrate NiIn (800 °C for 1 min) Ni/Au (750 °C for 1 min)
1 8.0 × 10−3 Ωcm2 1.2 × 10−2 Ωcm2
2 9.5 × 10 3 Ωcm2 2.1 × 10 2 Ωcm2

Figure 1(a) I-V behavior of NiIn/p-GaN contacts annealed at 800 °C for 1 min.

Figure 1(b) I-V behavior of NiIn/p-GaN contacts annealed at 750 °C for 1 min.

These electrical results show that NiIn has potential as an ohmic contact to p-GaN. However to understand the NiIn/p-GaN contacts, particularly its large resistance change upon annealing, will require careful interfacial characterization. At this time it is not clear what mechanism is responsible for the change in contact resistance due to annealing and the role oxidation may play in the measured resistance is equally unknown. It is this type of information, which is required not only to increase our understanding but also aid in the optimization of the NiIn contacts.

Conclusions

The intermetallic compound NiIn (50:50 at % ratio) was selected based on the criteria for the exchange mechanism as possible ohmic contacts to p-GaN. Contacts were fabricated on p-GaN films using RF sputtering from a compound target. In the as-deposited state these contacts were found to be rectifying and using I-V characterization a Schottky barrier height 0.82 eV was determined for the contact. Rapid thermal annealing of the NiIn contacts was shown to decrease their resistance with increasing annealing temperature. Contacts annealed at 800 °C for 1 min had the lowest resistance of the annealing conditions examined in this study. At this annealing condition the specific contact resistance of the NiIn contacts was measured to be 8 − 9 × 10−3 Ω cm2 using the circular TLM method. Annealing at higher temperatures or longer times resulted in an increase in specific contact resistance. It is speculated based upon Auger depth profiling that oxidation maybe responsible for this resistance increase at annealing conditions more severe than 800 °C for 1 min. The measured electrical properties of NiIn are promising since the specific contact resistance of NiIn is lower than the more traditionally used Ni/Au contact (ρc = 1.2 − 2.1 × 10−2 Ωcm2) processed under the same conditions.

Acknowledgements

The authors would like to thank Rick Schneider at the Hewlett-Packard Company for providing the p-GaN films used in this study and the National Science Foundation for its support of this project through grant number NSF-DMR-94-24478.

Footnotes

MRS Internet J. Nitride Semicond. Res. 4S1, G6.49(1999)

References

Morkoc, H., Strite, S., Gao, G. B., Lin, M. E., Sverdlov, B., and Burns, M., J. Appl. Phys. 76(3), 1363 (1994).Google Scholar
Morkoc, H. and Mohammad, S. N., Science 267, 51 (1995).Google Scholar
Pearton, S. J. and Kuo, C., MRS Bulletin 22, 17 (1997).CrossRefGoogle Scholar
Mori, T., Kozawa, T., Ohwaki, T., Taga, Y., Nagai, S., Yamasaki, S., Asami, S., Shibata, N. and Koike, M., Appl. Phys. Lett. 69(23), 3537 (1996).CrossRefGoogle Scholar
Nakamura, S., Senoh, M., Iwasa, N. and Nagahama, S., Jpn. J. Appl. Phys. 34, L797 (1995).Google Scholar
Trexler, J. T., Miller, S, J, Holloway, P. H. and Khan, M. A., Mater. Res. Soc. Sympo. Proc. 395, 819 (1996).Google Scholar
Kim, T., Yoo, M. C., and Kim, T., Mater. Res. Soc. Symp. Proc. 449, 1061 (1997).Google Scholar
King, D. J., Zhang, L., Ramer, J. C., Hersee, S. D., Lester, L. F., Mater. Res. Soc. Symp. Proc. 468, 421 (1997).Google Scholar
Smith, L. L., Davis, R. F., Kim, M. J., Carpenter, R. W. and Huang, Y., J. Mater. Res. 12, 2249 (1997).CrossRefGoogle Scholar
Trexler, J. T., Pearton, S. J., Holloway, P. H., Mier, M. G., Evans, K. R., and Karlicek, R. F., Mater. Res. Soc. Symp. Proc. 449, 1091 (1997).CrossRefGoogle Scholar
Soon, J. -S., Kim, H. –G., Park, K. –H., Um, C. –S., Han, I. -L., Kim, S. -H., Jang, H. –K., Park, S. –J., Mater. Res. Soc. Symp. Proc. 482, 1053 (1998).Google Scholar
Nakamura, S., Mater. Res. Soc. Symp. Proc. 482, 1145 (1998).Google Scholar
Venugopalan, H.S., Mohney, S.E., Luther, B. P., DeLucca, J. M., Wolter, S. D., Redwing, J. M., and Bulman, G. E., Mater. Res. Soc. Symp. Proc. 468, 431 (1997).CrossRefGoogle Scholar
Lin, C.-F., Chang, Y. A., Pan, N., Huang, J.-W., and Kuech, T.-F., Appl. Phys. Lett. 67, 3587 (1995).Google Scholar
Chen, D. Y., Chang, Y. A. and Swenson, D., Appl. Phys. Lett. 68, 96 (1996).Google Scholar
Chen, D.Y., Chang, Y. A. and Swenson, D., J. Appl. Phys. 81, 297 (1997).CrossRefGoogle Scholar
Chen, D. Y., Ph. D. Thesis, University of Wisconsin, Madison, WI (1997).Google Scholar
Swenson, D., Jan, C. -H., Chang, Y. A., J. Appl. Phys. 84, (1998).CrossRefGoogle Scholar
Okamoto, H., in Massalski, T. B. (ed.), Binary Alloy Phase Diagrams, ASM International, Materials Park, OH, 2276 (1990) 2nd edn.Google Scholar
Marlow, G. S. and Das, M. B., Solid-State Electronics 25, 91 (1982)CrossRefGoogle Scholar
Schroder, D. K., Semiconductor Material and Device Characterization, John Wiley and Sons, Inc, New York, NY, 151 (1990)Google Scholar
Ishikawa, H., Kobayashi, S., Koide, Y., Yamasaki, S., Nagai, S., Umezaki, J., Koike, M., and Murakami, M., J. Appl. Phys. 8 1(3), 1315 (1997).CrossRefGoogle Scholar
Tung, R.T., Vac, J.. Sci. Technol. B 11(4), 1546 (1993).Google Scholar
Figure 0

Table 1. Ideality factors and Schottky barrier height for as-deposited contacts

Figure 1

Table 2. Specific Contact Resistance for NiIn contacts

Figure 2

Table 3. A comparison of specific contact resistance NiIn Vs. Ni/Au

Figure 3

Figure 1(a) I-V behavior of NiIn/p-GaN contacts annealed at 800 °C for 1 min.

Figure 4

Figure 1(b) I-V behavior of NiIn/p-GaN contacts annealed at 750 °C for 1 min.