Hostname: page-component-cd9895bd7-7cvxr Total loading time: 0 Render date: 2024-12-27T05:36:35.143Z Has data issue: false hasContentIssue false

Photocatalytic Degradation of Methylene Blue Over Layered Double Hydroxides Using Various Divalent Metal Ions

Published online by Cambridge University Press:  01 January 2024

Guoxiang Pan*
Affiliation:
Department of Materials Engineering, Huzhou University, Huzhou 313000, People's Republic of China Zhejiang Huayuan Pigment Co., Ltd, Deqing 313220, People's Republic of China
Minhong Xu
Affiliation:
Department of Materials Engineering, Huzhou University, Huzhou 313000, People's Republic of China
Kai Zhou
Affiliation:
Department of Materials Engineering, Huzhou University, Huzhou 313000, People's Republic of China
Yue Meng
Affiliation:
Department of Materials Engineering, Huzhou University, Huzhou 313000, People's Republic of China
Haifeng Chen
Affiliation:
Department of Materials Engineering, Huzhou University, Huzhou 313000, People's Republic of China
Yuhua Guo
Affiliation:
Department of Materials Engineering, Huzhou University, Huzhou 313000, People's Republic of China
Tao Wu
Affiliation:
Department of Materials Engineering, Huzhou University, Huzhou 313000, People's Republic of China
*
*E-mail address of corresponding author: pgxzjut@163.com
Rights & Permissions [Opens in a new window]

Abstract

To apply hydrotalcites more effectively to the problem of dye wastewater, the effects of divalent metal ions on the structure and stability of hydrotalcites, especially on their photocatalytic activity, were compared. In the present study, M/Cr hydrotalcites (M3Cr-CO3-LDHs) (in which M = Mg, Co, Ni, Cu, Zn), where the M/Cr molar ratio was 3, were prepared by the co-precipitation method. The structures and properties were characterized using powder X-ray diffraction (XRD), Fourier-transform infrared spectroscopy (FTIR), thermogravimetric-differential thermal analysis (TG-DTA), and UV-Visible diffuse reflectance spectroscopy (UV-Vis DRS). The results showed that five kinds of M3Cr-CO3-LDHs were synthesized successfully, and the layered structure of the samples obtained was regular and the crystal phase was single. When methylene blue (MB) solution was exposed to ZnCr-CO3-LDHs, H2O2, and visible light irradiation, more than 90.67% of the methylene blue (MB) was removed after 140 min. The photocatalytic activity of the samples was in the order: Co3Cr-CO3-LDHs > Mg3Cr-CO3-LDHs > Cu3Cr-CO3-LDHs > Zn3Cr-CO3-LDHs > Ni3Cr-CO3-LDHs. The results of a catalytic mechanism study showed that photocatalytic degradation of MB involved a demethylation reaction, with the reactive species containing •O2-, •OH, and h+.

Type
Article
Copyright
Copyright © Clay Minerals Society 2019

Introduction

Dye wastewater is industrial waste which is difficult to deal with because of its high concentration, poor biodegradability, and high chromaticity (Xia et al. Reference Xia, Liu, Ni, Shi, Xue and Qian2014; Kuzyaka et al. Reference Kuzyaka, Galioglu, Altın, Sökmen and Akata2018). With the rapid development of printing and dyeing industries, the increase in wastewater emissions has led to a sharp decline in water quality in the natural environment (Shang et al. Reference Shang, Xi, Liu, Tan, Chen, Wu and Pan2017). In addition, if dye wastewater is discharged to the environment without timely treatment, a series of chemical reactions is generated which produces toxic by-products, which worsen the ecological situation (Crossland et al. Reference Crossland, Noel, Sivaram, Leijtens, Alexander-Webber and Snaith2013; Alijani et al. Reference Alijani, Kaleji and Rezaee2017; Bohac & Bujdak Reference Bohac and Bujdak2018; Karataş et al. Reference Karataş, Senol-Arslan and Ozdemir2018). Photocatalytic degradation is a relatively recent technology which is showing significant potential in terms of its ability to control pollution (Ray et al. Reference Ray, Dhakal, Kshetri and Lee2017; Adeleke et al. Reference Adeleke, Theivasanthi, Thiruppathi, Swaminathan, Akomolafe and Alabi2018). Identifying efficient catalysts for organic dye wastewater treatment is vitally important.

Hydrotalcites are anionic layered clay materials (layered double hydroxides, LDHs) and the molecular formula of a typical hydrotalcite-like compound is Mg6Al2(OH)16CO3·4H2O. Mg2+ and Al3+ in LDHs can be replaced in the structure isomorphously by other divalent and trivalent cations (Zhou et al. Reference Zhou, Li, Ai, Tian and Hong2016). The general formula of the compound is [M 2+1–x M 3+ x (OH)2] x+(A n) x/n ·mH2O, in which A n represents interlayer anions, x is the ratio M 3+/(M 2++M 3+), and m is the quantity of crystal water (Pan et al. Reference Pan, Ni, Cao and Li2012; Vialat et al. Reference Vialat, Leroux, Taviot-Gueho, Villemure and Mousty2013). Because LDHs have an exchangeable anion structure, adjustable pore size, thermal stability, and other properties, it can be used in catalysis, medicine, and other industries (Zhou & Keeling Reference Zhou and Keeling2013; Gao et al. Reference Gao, Sasaki and Qiu2018; Li et al. Reference Li, Yu, Altaf, Zhu, Li, Dai and Wang2018) New types of hydrotalcite have been synthesized by changing the metal cations and anions in the hydrotalcite structure, such as Mg/Al/Ce LDHs, Cu-Mg-Al LDHs, and Mg-Al LDHs doped with Tb etc. (Wang et al. Reference Wang, Wang, Dong, Zhang, Pei, Chen and Jin2011; Chen et al. Reference Chen, Bao and Wang2016; Comelli et al. Reference Comelli, Ruiz, Aparicio, Merino and Ponzi2018; Xu et al. Reference Xu, Pan, Meng, Guo, Wu and Chen2019). Research into the application of photocatalytic activity of LDHs has become important (Zhou Reference Zhou2010; Zhang et al. Reference Zhang, Wang, Zhou, Ni and Xia2018). Photocatalytic degradation of pesticides was studied by Da et al. (Reference Da, Prevot, Forano, Wong-Wah-Chung, Burrows and Sarakha2014) using decatungstate intercalated macroporous layered double hydroxides. Visible light-promoted degradation of gaseous volatile organic compounds catalyzed by Au supported on layered double hydroxides was studied by Fu et al. (Reference Fu, Zheng, Zhou, Ni and Xia2019).

In order to evaluate the exchangeability of cations on hydrotalcite laminates (Mao et al. Reference Mao, Zhou, Tong, Yu and Cynthia Lin2017) and to maximize the potential of hydrotalcites in the dye wastewater treatment, the effects of divalent metal ions on the structure, stability, and photocatalytic activity of hydrotalcites were assessed. To this end, M/Cr hydrotalcite (M 3Cr-CO3-LDHs, where M = Mg, Co, Ni, Cu, or Zn), with an M/Cr atomic ratio of 3, was prepared by the co-precipitation method. Photocatalytic performance is assessed by measuring the degradation of MB aqueous solutions under visible irradiation. The effects of irradiation time, catalyst type, and reuse performance of MB degradation were investigated and the reaction mechanism was studied also.

Experimental

Materials

For the present study, analytically pure M(NO3)2·6H2O (M is Co, Mg, Ni, Zn, Cu), Cr(NO3)3·9H2O, Na2CO3, NaOH, isopropanol, p-benzoquinone, ethylene diamine tetraacetic acid disodium salt, H2O2, and MB were purchased from Aladdin Reagent Co., Ltd (Shanghai, China). All solutions were prepared with deionized water.

Preparation of M3Cr-CO3-LDHs

A series of M 3Cr-CO3-LDHs was synthesized employing the co-precipitation method (Pan et al. Reference Pan, Ni, Cao and Li2012). Using a M/Cr molar ratio of 3.0, known amounts of M(NO3)2·6H2O and Cr(NO3)3·9H2O solid were dissolved in boiling water to be used as solution A. Then, 6.40 g of NaOH and 1.06 g of Na2CO3 were dissolved in boiling water as solution B. Under constant stirring, solutions A and B were added drop-wise to a beaker which was filled with deionized water. In this process, the mixed solution was adjusted using NaOH solution until the pH was between 9 and 10. The solution was then stirred continuously for 30 min. Finally, the slurry obtained was aged at 65°C for 24 h. The resulting precipitates were centrifuge washed with deionized water. After that, the samples were dried overnight at 65°C, and they were labeled using the format M 3Cr-CO3-LDH.

Structural Characterization

X-ray diffraction patterns of the samples were recorded an XD-6 instrument using CuKα radiation (Beijing Purkinje General Instrument Co., Ltd., Beijing, China). Infrared spectra were recorded using the KBr disc method on a Nicolet 5700 FTIR spectrophotometer (Thermo Scientific, Waltham, Massachusetts, USA). The thermal properties of the samples were measured using a CRY-2P instrument (Beijing Henven scientific instrument factory, Beijing, China); the heating rate was 10°C/min and the temperature range was 25–800°C. UV-Vis diffuse reflectance spectra (UV-Vis DRS) of the samples were tested using a UV4100 UV-Vis spectrophotometer (Thermo Scientific, Waltham, Massachusetts, USA); BaSO4 was used as a reference standard. The time-dependent UV-Vis spectra of MB solutions were measured using a Shimadzu UV-2600 UV-Vis spectrophotometer (Tokyo, Japan).

Catalytic Experiments

The photocatalytic properties of ZnCr-CO3-LDHs were determined by photodegradation of MB solution under visible light irradiation using a 150 W halogen lamp. A photocatalyst (0.5 g) was mixed with 25 mL of 5 mg/L MB aqueous solution with an additional 0.5 mL of H2O2. The mixed solution was stirred with a magnetic stirrer. A sample solution was taken at a given time and separated through centrifugation. The concentration of MB solution was evaluated by UV-Vis spectrophotometry at 662 nm. The degradation efficiency was calculated using the following equation:

D = C 0 C t / C 0 × 100 = A A t / A × 100 %

where C 0 is the initial concentration of MB solution after avoiding light, and C t is the concentration of MB solution after a known photoreaction time, A is the initial absorbance of MB solution after avoiding light, and A t is the absorbance of MB solution after a known photoreaction time.

Results and Discussion

XRD Characterization

The regularity of the crystal structure, crystallinity, and crystal-cell parameters of the samples was tested using XRD (Chen et al. Reference Chen, Bao and Wang2016). The XRD patterns of five kinds of M 3Cr-CO3-LDHs (Fig. 1) showed that the diffraction peaks were at 11.7, 23.6, and 34.7°2θ, which corresponded to the characteristic diffraction peaks of hydrotalcite; and the crystal face indexes were (003), (006), and (009), respectively. The above-mentioned results were consistent with published information (Prevot et al. Reference Prevot, Forano and Besse2005; Pan et al. Reference Pan, Cao, Ni, Li, Chen, Tang and Xu2011; Yang et al. Reference Yang, Qian, Chu and Zhang2018; Xu et al. Reference Xu, Pan, Meng, Guo, Wu and Chen2019), indicating that the five kinds of M 3Cr-CO3-LDHs had typical layered structures. The diffraction peaks of these five kinds of M 3Cr-CO3-LDHs were strong and sharp, which indicated that the synthesized M 3Cr-CO3-LDHs had fine crystallinity. In addition, the diffraction peak of Zn3Cr-CO3-LDHs was the strongest, which showed that Zn3Cr-CO3-LDHs formed the best crystals. The peak observed at d 009 in Cu3Cr-CO3-LDHs, however, was unidentified and indicated less crystallinity. It may have been a consequence of incomplete washing.

Fig. 1 XRD patterns of Mg3Cr-CO3-LDHs (a), Co3Cr-CO3-LDHs (b), Ni3Cr-CO3-LDHs (c), Cu3Cr-CO3-LDHs (d), and Zn3Cr-CO3-LDHs (e)

The layer spacing of the diffraction peak corresponding to the d 003 plane was calculated from the Bragg equation (nλ = 2dsinθ), giving values for CuCr-CO3-LDHs, ZnCr-CO3-LDHs, NiCr-CO3-LDHs, MgCr-CO3-LDHs, and CoCr-CO3-LDHs of 0.747, 0.764, 0.773, 0.765, and 0.749 nm, respectively. These data are similar to the results reported in the literature of d 003 spacing of carbonate hydrotalcite (Sels et al. Reference Sels, De Vos and Jacobs2001; Rives et al. Reference Rives, Prieto, Dubey and Kannan2003; Tichit et al. Reference Tichit, Gerardin, Durand and Coq2006; Yang et al. Reference Yang, Chu and Zhang2019). Comparison of the five d 003 results revealed that the MgCr-CO3-LDHs layer spacing was the largest, which might be due to the fact that Mg has the smallest atomic radius.

FTIR Spectroscopy Analysis

The FTIR patterns of the five kinds of M 3Cr-CO3-LDHs (Fig. 2) revealed five absorption peaks between 3470 and 3540 cm–1 which were ascribed to the stretching vibration of the H2O molecule; this was because the surface and the interlayer space of the LDHs adsorbed a certain number of H2O molecules. Compared with the stretching vibration of free hydroxyl (at ~3650 cm–1), the peak shifted to a lower wavenumber, which indicated that a hydrogen bond between layers of H2O and the CO3 2– ion and the hydroxyl group appeared. In addition, absorption peaks between 1650 and 1665 cm–1 were caused by the bending vibration of –OH in the crystal water. The peak at 1384–1386 cm–1 was ascribed to the anti-symmetric stretching vibration peak of CO3 2–. Absorption peaks between 520 and 630 cm–1 belonged to the characteristic peak of plane-bending vibration of C-O. All the patterns showed the characteristic peaks of hydrotalcite. IR spectra further confirmed the synthesis of M 3Cr-CO3-LDHs had typical structural characteristics of hydrotalcite.

Fig. 2 FTIR patterns of Mg3Cr-CO3-LDHs (a), Co3Cr-CO3-LDHs (b), Ni3Cr-CO3-LDHs (c), Cu3Cr-CO3-LDHs (d), and Zn3Cr-CO3-LDHs (e)

TG-DTA Characterization

The TG-DTA curves of Mg3Cr-CO3-LDHs, Zn3Cr-CO3-LDHs, Co3Cr-CO3-LDHs, Ni3Cr-CO3-LDHs, and Cu3Cr-CO3-LDHs (Fig. 3a) showed that during the heating process, the thermal behavior of these compounds could be divided into two stages. In the first stage, the weight loss was ~17–25%, and in the second stage, weight loss was ~17–23%. Compared with the five kinds of compounds, Mg3Cr-CO3-LDHs had the largest weight loss: 23%. The comparison of DTA curves showed that the thermal decomposition of the five kinds of M 3Cr-CO3-LDHs was due mainly to two obvious endothermic processes. An endothermic peak appeared at low temperature (i.e. 50–200°C), which corresponded to the removal of surface-adsorbed water and interlayer water. A peak also appeared at higher temperature (i.e. 265–450°C), indicating that the interlayer hydroxyl was dehydrated and interlayer CO3 2– anions were decomposed or removed. These results were similar to the thermal decomposition of typical Mg-Al hydrotalcites (Hibino et al. Reference Hibino, Yamashita, Kosuge and Tsunashima1995).

Fig. 3 TG curves of of M 3Cr-CO3-LDHs (a), and DTA curves of M 3Cr-CO3-LDHs (b)

Comparison of second-stage DTA curves (Fig. 3b) indicated the thermal decomposition temperature of Cu3Cr-CO3-LDHs was the highest, which showed that the thermal stability was the best. The relative thermal stabilities of the other four kinds of hydrotalcites were in the order: Mg3Cr-CO3-LDHs > Ni3Cr-CO3-LDHs > Zn3Cr-CO3-LDHs ≈ Co3Cr-CO3-LDHs, consistent with the result reported previously (Pan et al. Reference Pan, Ni, Cao and Li2012), i.e. the order of thermal stability of hydrotalcites obtained from the second law of crystal chemistry.

UV-Vis DRS Analysis

The UV-Vis DRS spectra of LDHs (Fig. 4) showed that Mg3Cr-CO3-LDHs and Ni3Cr-CO3-LDHs (curve a and curve c) contained obvious absorption peaks at ~333 and 480 nm. Co3Cr-CO3-LDHs (curve b) had a weak absorption peak in the visible region (λ > 400 nm), but Cu3Cr-CO3-LDHs (curve d) had almost no absorption peaks, while Zn3Cr-CO3-LDHs (curve e) had obvious absorption peaks at ~410 and 560 nm. In order to utilize these kinds of catalysts effectively in visible light (λ > 400 nm), UV-Vis DRS patterns of the five kinds M 3Cr-CO3-LDHs were compared and analyzed. The absorption region of Zn3Cr-CO3-LDHs was widest, next was Ni3Cr-CO3-LDHs, and Mg3Cr-CO3-LDHs and Co3Cr-CO3-LDHs had narrower spectra, while the absorption region of Cu3Cr-CO3-LDHs was narrowest. With the various divalent metal cations, the final products were different colors (Zhao et al. Reference Zhao, Zhang, Li, Yan, He, Tian and Duan2011), meaning that their absorption of visible light spanned different wavelengths and provided an incentive to explore their visible-light catalytic properties.

Fig. 4 UV-Vis DRS patterns of Mg3Cr-CO3-LDHs (a), Co3Cr-CO3-LDHs (b), Ni3Cr-CO3-LDHs (c), Cu3Cr-CO3-LDHs (d), and Zn3Cr-CO3-LDHs (e)

Photocatalytic Properties of ZnCr-CO3-LDHs

In order to investigate the catalytic activity of ZnCr-CO3-LDHs, MB solution was selected as the substrate for catalytic oxidation. The removal rate of MB was only 5% in the presence of ZnCr-CO3-LDHs without visible light (Fig. 5), which was attributed to the adsorption capability of ZnCr-CO3-LDHs (for MB). In the presence of ZnCr-CO3-LDHs exposed to visible light, the removal rate was 10.06% after 140 min, indicating that ZnCr-CO3-LDHs is a photocatalyst for MB degradation. When both ZnCr-CO3-LDHs and H2O2 were involved in an unilluminated reaction, the removal rate of MB was 46.36% after 140 min. However, MB decreased by 49.08% when using only H2O2 for 140 min under visible light irradiation, which might be due to oxidation of H2O2. When MB solution was exposed to ZnCr-CO3-LDHs, H2O2, and visible light irradiation together, >90.67% of MB was removed after 140 min. The above phenomena indicated that MB was most effectively degraded by ZnCr-CO3-LDHs/H2O2 under visible light irradiation.

Fig. 5 Photocatalytic degradation of MB under various conditions

Reuse Performance

Repeated experiments on photodegradation of MB using ZnCr-CO3-LDHs/H2O2 were performed. After each run, the photocatalysts were collected by centrifugation; distilled water was added to the centrifuge tube and stirred until the catalyst was washed washed thoroughly, and then centrifugation was continued. The process was repeated three times. After the ZnCr-CO3-LDHs were reused three times, the degradation rates of MB solution were still >90% (Fig. 6), indicating that ZnCr-CO3-LDHs were stable and not photocorroded during photocatalytic reactions. In addition, when the photocatalysts were used for the second or third times, the MB was degraded rapidly. The photocatalytic degradation rate of MB was 42.65% (second attempt) and 42.14% (third attempt) after 20 min, which was faster than that of the first time of photocatalytic degradation of MB (17.76%).

Fig. 6 Catalyst recycling study of ZnCr-CO3-LDHs for photocatalytic degradation of MB

The quicker degradation might be due to the transition of electrons in the valence band when using ZnCr-CO3-LDHs in the presence of light, resulting in the formation of photogenerated electron-hole pairs on the inside and on the surface of ZnCr-CO3-LDHs. Electrons and holes reacted with H2O2 to produce active species that effectively prevented recombination of electron-hole pairs, and effectively transferred electrons and holes, resulting in a series of redox reactions. In the process of reuse, visible light irradiation may activate ZnCr-CO3-LDHs to produce photogenerated electron-hole pairs. Therefore, the reaction of photogenerated electrons and holes with H2O2 was accelerated and, ultimately, the degradation of MB was also accelerated.

The XRD patterns of ZnCr-CO3-LDHs after different cycles (Fig. 7) showed that the diffraction peaks of ZnCr-CO3-LDHs were unchanged and the peaks were similar in shape when ZnCr-CO3-LDHs were used two or three times. The results indicated that the crystal structure of hydrotalcites did not change obviously after cyclic use, and also proved that ZnCr-CO3-LDHs had good stability.

Fig. 7 XRD patterns of ZnCr-CO3-LDHs after various cycle times

Catalyst Types

The photocatalytic degradation of MB with different metal ions substituted in MCr-CO3-LDHs (M = Zn, Mg, Co, Ni, or Cu) (Fig. 8) showed that, under the same experimental conditions, the degradation of MB with CoCr-CO3-LDHs after 60 min was nearly 100%, while the degradation with MgCr-CO3-LDHs and CuCr-CO3-LDHs was >90%. But the degradation efficiencies of ZnCr-CO3-LDHs and NiCr-CO3-LDHs were worse; the degradation of MB was 55.78% and 48.14%, respectively, under the same conditions. When M was Mg, Co, or Cu, MB degraded rapidly, and a large number of bubbles was produced during the reaction. When M was Zn or Ni, fewer bubbles were formed. The photocatalytic activity of five kinds of M 3Cr-CO3-LDHs was in the order: Co3Cr-CO3-LDHs > Mg3Cr-CO3-LDHs > Cu3Cr-CO3-LDHs > Zn3Cr-CO3-LDHs > Ni3Cr-CO3-LDHs.

Fig. 8 Effect of catalyst types on degradation of MB

Photocatalytic Mechanism

The intermediate products of MB degradation were tested (Fig. 9); the maximum absorption peak (λ = 664 nm) of MB solution decreased gradually with the prolongation of reaction time, and the maximum absorption peak shifted to λ = 651 nm. The blue shift (to lower wavelengths) of the maximum absorption wavelength of MB occurred, possibly due to the demethylation reaction found when photocatalytic degradation of MB takes place, and it removed a methyl to form azure B. According to the literature (Zhang et al. Reference Zhang, Oyama, Aoshima, Hidaka, Zhao and Serpone2001), absorption bands at 654–648, 620, and 610 nm are due to MB molecular transformations to azure A, azure B, and azure C, respectively. The results of photocatalytic degradation of MB agreed with those reported in the literature. In addition, along with the prolonged irradiation time, a new absorption peak appeared in the UV region (λ = 372 nm); the absorption peak was enhanced as illumination time increased, suggesting that new substances appeared during degradation of MB.

Fig. 9 UV-Vis absorption spectra of MB with different reaction times in the presence of ZnCr-CO3-LDHs/H2O2 under visible light irradiation.

In order to evaluate the role of these active oxidants, scavengers were added to the photocatalytic system. These were isopropanol (IPA) for •OH, p-benzoquinone (BQ) for •O2 (Yuan et al. Reference Yuan, Wei, Hu, Yao, Jiang, Fang and Chu2015), and ethylene diamine tetraacetic acid disodium salt (EDTA-2Na) for h + (Xiong et al. Reference Xiong, Chen, He, Sun and Wang2012; Pan et al. Reference Pan, Wang, Sun, Xu and Wang2013; Chen et al. Reference Chen, He, Lv, Liu, Wang and Lv2014). The molar ratio of initial concentration of these three kinds of scavengers in the reaction system to MB was 200:1. The photodegradation of MB was slightly inhibited by the addition of IPA (Fig. 10). The results indicated that MB degradation was driven mainly by the participation of •OH radicals. But the reaction was accelerated when EDTA-2Na and BQ were added. The degradation rates of MB exceeded 90% after irradiation for 60 min.

Fig. 10 Effect of various scavengers on degradation of MB

Based on the band theory of solids and the mechanism of semiconductor photocatalysis, researchers speculated on the possible mechanism of photocatalytic degradation of MB. Photoinduced e /h + pairs were generated on the surface of the photocatalyst ZnCr-CO3-LDHs during irradiation (Eq. 1). H2O2 molecules oxidized by photoinduced h + were adsorbed into •OH species on the photocatalyst surface (Eq. 2), while the photoinduced e -activated H2O2 and O2 molecules were adsorbed into •OH, OH species on the catalyst surface (Eq. 3), and •O2 species (Eq. 4), respectively. In addition, •OH species were also generated during irradiation of H2O2 (Eq. 5). H2O2 oxidized the active •O2 species into •OH, OH, and O2 species (Eq. 6). •OH and O2 species are known to be the main active species in the photocatalytic reaction (Ishibashi et al. Reference Ishibashi, Fujishima, Watanabe and Hashimoto2000; Xiang et al. Reference Xiang, Yu and Wong2011). The MB molecules were oxidized by •OH and O2 species into small molecules (Eq. 7 and Eq. 8).

(1) ZnCr CO 3 LDHs + h v e + h +
(2) h + + H 2 O 2 2 OH
(3) e + H 2 O 2 OH + OH
(4) e + O 2 O 2
(5) H 2 O 2 + h v 2 OH
(6) O 2 + H 2 O 2 OH + OH + O 2
(7) OH + MB Degradation products
(8) O 2 + MB Degradation products

When the EDTA-2Na was added to the reaction system, the h + was captured, which caused Eq. 1 to move to the right, so that a large amount of photoinduced e formed on the catalyst surface and inside. Photoinduced e deoxidizes H2O2 and O2 molecules to produce •OH and •O2 species on the photocatalyst surface according to Eq. 3 and Eq. 4. The •OH could oxidize MB effectively, while •O2 and H2O2 generated •OH and O2 according to Eq. 6. Therefore, in the process of photocatalysis of MB, a large number of bubbles were produced in the solution, and the MB was degraded rapidly. When p-benzoquinon was added, •O2 in the solution was trapped, which caused Eq. 4 to move to the right. Subsequently, Eq. 1 and Eq. 2 were accelerated, speeding up the generation of •OH and accelerating the degradation of MB. However, one could speculate that the addition of p-benzoquinon did not capture •O2 rapidly, so that part of •O2 could react with H2O2 (Eq. 6). This concept is consistent with the fact that a large number of bubbles was produced in the solution during the experiment.

Based on the above discussion, combined with the analysis of UV-Vis absorption spectra, the possible mechanism of ZnCr-CO3-LDHs photocatalytic degradation of MB was considered (Fig. 11). Under visible light irradiation, ZnCr-CO3-LDH was excited, and its valence band electrons were transferred to the conduction band to produce photogenerated electrons (e ) and holes (h +). These e and h + could move freely in the catalyst. When they moved to the catalyst surface, e reacted with O2 and H2O2 in the solution to produce •O2 and •OH, and h + in the valence band reacted with H2O2 to generate •OH. These active species then reacted with MB, causing MB to undergo demethylation, and also oxidized MB to small molecules, thus achieving the purpose of decolorization and degradation.

Fig. 11 Possible mechanism of photocatalytic degradation of MB using ZnCr-CO3-LDHs

Conclusions

In the present study, M/Cr hydrotalcites (M 3Cr-CO3-LDHs) (in which M = Mg, Co, Ni, Cu, or Zn), where the M/Cr molar ratio was 3, were prepared by the co-precipitation method. XRD and FTIR tests showed that five kinds of M 3Cr-CO3-LDHs were synthesized successfully, the samples obtained had regular layered structures and were single crystal phases. FTIR and TG-DTA analysis showed the M 3Cr-CO3-LDHs to have thermal stability characteristics typical of carbonate hydrotalcites. In addition, the thermal stability was in the order: Cu3Cr-CO3-LDHs > Mg3Cr-CO3-LDHs > Ni3Cr-CO3-LDHs > Zn3Cr-CO3-LDHs ≈ Co3Cr-CO3-LDHs. When MB solution was exposed to ZnCr-CO3-LDH, H2O2, and visible light irradiation together, more than 90.67% of the MB was removed after 140 min. Photocatalytic activity of the samples was in the order: Co3Cr-CO3-LDHs > Mg3Cr-CO3-LDHs > Cu3Cr-CO3-LDHs> Zn3Cr-CO3-LDHs >Ni3Cr-CO3-LDHs. The results of a reaction mechanisms study showed photocatalytic degradation of MB involved demethylation, and the reactive species contained •O2 -, •OH, and h +.

Acknowledgements

This Project is supported by Zhejiang Provincial Natural Science Foundation of China (No. LY17E040001; No. LQ19E040001).

Footnotes

This paper was originally presented during the World Forum on Industrial Minerals, held in Qing Yang, China, October 2018.

AE: Chun-Hui Zhou

References

Adeleke, J. T. Theivasanthi, T. Thiruppathi, M. Swaminathan, M. Akomolafe, T. Alabi, A. B., Photocatalytic degradation of methylene blue by ZnO/NiFe2O4 nanoparticles Applied Surface Science 2018 455 195200 10.1016/j.apsusc.2018.05.184.CrossRefGoogle Scholar
Alijani, M. Kaleji, B. K. Rezaee, S., Highly visible-light active with Co/Sn co-doping of TiO2 nanoparticles for degradation of methylene blue Journal of Materials Science Materials in Electronics 2017 28 1534515353 10.1007/s10854-017-7420-6.CrossRefGoogle Scholar
Bohac, P. Bujdak, J., Prepublication: tuning the photophysical properties of cyanine dyes with clay minerals Clays and Clay Minerals 2018 66 127137 10.1346/CCMN.2018.064090.CrossRefGoogle Scholar
Chen, Q. He, Q. Q. Lv, M. M. Liu, X. T. Wang, J. Lv, J. P., The vital role of PANI for the enhanced photocatalytic activity of magnetically recyclable N–K2Ti4O9/MnFe2O4/PANI composites Applied Surface Science 2014 311 230238 10.1016/j.apsusc.2014.05.046.CrossRefGoogle Scholar
Chen, Y. F. Bao, Y. Wang, X. Q., Green emission of Tb-doped Mg-Al layered double hydroxide response to L-lysine Journal of Fluorescence 2016 26 813820 10.1007/s10895-016-1769-4.CrossRefGoogle ScholarPubMed
Comelli, N. A. Ruiz, M. L. Aparicio, MSL Merino, N. A. Ponzi, M. I., Influence of the synthetic conditions on the composition, morphology of cumgal hydrotalcites and their use as catalytic precursor in diesel soot combustion reactions Applied Clay Science 2018 157 148157 10.1016/j.clay.2018.02.039.CrossRefGoogle Scholar
Crossland, EJW Noel, N. Sivaram, V. Leijtens, T. Alexander-Webber, J. A. Snaith, H. J., Mesoporous TiO2 single crystals delivering enhanced mobility and optoelectronic device performance Nature 2013 495 215219 10.1038/nature11936.CrossRefGoogle ScholarPubMed
Da, S. E. Prevot, V. Forano, C. Wong-Wah-Chung, P. Burrows, H. D. Sarakha, M., Heterogeneous photocatalytic degradation of pesticides using decatungstate intercalated macroporous layered double hydroxides Environmental Science & Pollution Research International 2014 21 1121811227 10.1007/s11356-014-2971-z.Google Scholar
Fu, S. Zheng, Y. Zhou, X. Ni, Z. Xia, S., Visible light promoted degradation of gaseous volatile organic compounds catalyzed by au supported layered double hydroxides: influencing factors, kinetics and mechanism Journal of Hazardous Materials 2019 363 4154 10.1016/j.jhazmat.2018.10.009.CrossRefGoogle ScholarPubMed
Gao, Z. Sasaki, K. Qiu, X., Structural memory effect of Mg-Al and Zn-Al layered double hydroxides in the presence of different natural humic acids: process and mechanism Langmuir 2018 34 53865395 10.1021/acs.langmuir.8b00059.CrossRefGoogle ScholarPubMed
Hibino, T. Yamashita, Y. Kosuge, K. Tsunashima, A., Decarbonation behavior of Mg-Al-CO3 hydrotalcite-like compounds during heat treatment Clays and Clay Minerals 1995 43 427432 10.1346/CCMN.1995.0430405.CrossRefGoogle Scholar
Ishibashi, K. Fujishima, A. Watanabe, T. Hashimoto, K., Quantum yields of active oxidative species formed on TiO2, photocatalyst Journal of Photochemistry & Photobiology A Chemistry 2000 134 139142 10.1016/S1010-6030(00)00264-1.CrossRefGoogle Scholar
Karataş, D˙z Senol-Arslan, D. Ozdemir, O., Experimental and atomic modeling of the adsorption of acid azo dye 57 to sepiolite Clays and Clay Minerals. 2018 66 426437 10.1346/CCMN.2018.064109.CrossRefGoogle Scholar
Kuzyaka, D. Galioglu, S. Altın, İ Sökmen, M. Akata, B., The effect of microporous vanadosilicate Am-6 thin films as photocatalysts for the degradation of methylene blue Journal of Photochemistry & Photobiology A Chemistry 2018 366 127135 10.1016/j.jphotochem.2018.03.041.CrossRefGoogle Scholar
Li, P. Yu, F. Altaf, N. Zhu, M. Li, J. Dai, B. Wang, Q., Two-dimensional layered double hydroxides for reactions of methanation and methane reforming in C1 Chemistry Materials 2018 11 221246 10.1016/j.electacta.2017.12.139.CrossRefGoogle ScholarPubMed
Mao, N. Zhou, C. H. Tong, D. S. Yu, W. H. Cynthia Lin, C. X., Exfoliation of layered double hydroxide solids into functional nanosheets Applied Clay Science 2017 144 6078 10.1016/j.clay.2017.04.021.CrossRefGoogle Scholar
Pan, G. X. Cao, F. Ni, Z. M. Li, X. N. Chen, H. F. Tang, P. S. Xu, M. H., Preparation of NiMgAl layered double hydroxides and hydrogen production from aqueous-phase reforming of ethylene glycol Journal of the Chinese Ceramic Society 2011 39 585589 10.5535/arm.2011.35.3.427.Google Scholar
Pan, G. X. Ni, Z. M. Cao, F. Li, X. N., Hydrogen production from aqueous-phase reforming of ethylene glycol over Ni/Sn/Al hydrotalcite derived catalysts Applied Clay Science 2012 58 108113 10.1016/j.clay.2012.01.023.CrossRefGoogle Scholar
Pan, X. Wang, L. J. Sun, X. Q. Xu, B. H. Wang, X., Ternary Titania–Cobalt Ferrite–polyaniline nanocomposite: a magnetically recyclable hybrid for adsorption and photodegradation of dyes under visible light Industrial & Engineering Chemistry Research 2013 52 1010510113 10.1021/ie400739e.Google Scholar
Prevot, V. Forano, A. Besse, J. P., Hydrolysis in polyol: new route for hybrid-layered double hydroxides preparation Chemistry of Materials 2005 17 66956701 10.1021/cm050581x.CrossRefGoogle Scholar
Ray, S. K. Dhakal, D. Kshetri, Y. K. Lee, S. W., Cu-α-NiMoO4 photocatalyst for degradation of Methylene blue with pathways and antibacterial performance Journal of Photochemistry & Photobiology A Chemistry 2017 348 1832 10.1016/j.jphotochem.2017.08.004.CrossRefGoogle Scholar
Rives, V. Prieto, O. Dubey, A. Kannan, S., Synergistic effect in the hydroxylation of phenol over CoNiAl ternary hydrotalcites Journal of Catalysis 2003 220 161171 10.1016/S0021-9517(03)00245-8.CrossRefGoogle Scholar
Sels, B. F. De Vos, D. E. Jacobs, P. A., Hydrotalcite-like anionic clays in catalytic organic reactions Catalysis Reviews 2001 43 443488 10.1081/CR-120001809.CrossRefGoogle Scholar
Shang, Y. Xi, C. Liu, W. Tan, P. Chen, H. Wu, L. Pan, J., Photocorrosion inhibition and high-efficiency photoactivity of porous g-C3N4/Ag2CrO4 composites by simple microemulsion-assisted co-precipitation method Applied Catalysis B Environmental 2017 204 7888 10.1016/j.apcatb.2016.11.025.CrossRefGoogle Scholar
Tichit, D. Gerardin, C. Durand, R. Coq, B., Layered double hydroxides: precursors for multifunctional catalysts Topics in Catalysis 2006 39 8996 10.1007/s11244-006-0041-6.CrossRefGoogle Scholar
Vialat, P. Leroux, F. Taviot-Gueho, C. Villemure, G. Mousty, C., Insights into the electrochemistry of (CoxNi(1−x))2Al–NO3 layered double hydroxides Electrochimica Acta 2013 107 599610 10.1016/j.electacta.2013.06.033.CrossRefGoogle Scholar
Wang, L. Wang, D. Dong, X. Y. Zhang, Z. J. Pei, X. F. Chen, X. J. Jin, J. A., Layered assembly of graphene oxide and Co-Al layered double hydroxide nanosheets as electrode materials for supercapacitors Chemical Communications 2011 47 35563668 10.1039/c0cc05420h.CrossRefGoogle ScholarPubMed
Xia, S. J. Liu, F. X. Ni, Z. M. Shi, W. Xue, J. L. Qian, P. P., Ti-based layered double hydroxides: efficient photocatalysts for azo dyes degradation under visible light Applied Catalysis B: Environmental 2014 144 570579 10.1016/j.apcatb.2013.07.060.CrossRefGoogle Scholar
Xiang, Q. Yu, J. Wong, P. K., Quantitative characterization of hydroxyl radicals produced by various photocatalysts Journal of Colloid & Interface Science 2011 357 163167 10.1016/j.jcis.2011.01.093.CrossRefGoogle ScholarPubMed
Xiong, P. Chen, Q. He, M. Y. Sun, X. Q. Wang, X., Cobalt ferrite–polyaniline heteroarchitecture: a magnetically recyclable photocatalyst with highly enhanced performances Journal of Materials Chemistry 2012 22 1748517493 10.1039/C2JM31522J.CrossRefGoogle Scholar
Xu, M. Pan, G. Meng, Y. Guo, Y. Wu, T. Chen, H., Effect of Ce3+ on the photocatalytic activity of MAlCe ternary hydrotalcites-like compounds in methylene blue photodegradation Applied Clay Science 2019 170 4656 10.1016/j.clay.2019.01.011.CrossRefGoogle Scholar
Yang, Z. H. Qian, W. M. Chu, Y. M. Zhang, W., On approximating the arithmetic-geometric mean and complete elliptic integral of the first kind Journal of Mathematical Analysis and Applications 2018 462 17141726 10.1016/j.jmaa.2018.03.005.CrossRefGoogle Scholar
Yang, Z. H. Chu, Y. M. Zhang, W., High accuracy asymptotic bounds for the complete elliptic integral of the second kind Applied Mathematics and Computation 2019 348 552564 10.1016/j.amc.2018.12.025.CrossRefGoogle Scholar
Yuan, B. Wei, J. Hu, T. Yao, H. B. Jiang, Z. H. Fang, Z. W. Chu, Z. Y., Simple synthesis of g-C3N4/rGO hybrid catalyst for the photocatalytic degradation of rhodamine B Chinese Journal of Catalysis 2015 36 10091016 10.1016/S1872-2067(15)60844-0.CrossRefGoogle Scholar
Zhang, T. Y. Oyama, T. Aoshima, A. Hidaka, H. Zhao, J. C. Serpone, N., Photooxidative n-demethylation of methylene blue in aqueous TiO2 dispersions under UV irradiation Journal of Photochemistry & Photobiology A Chemistry 2001 140 163172 10.1016/S1010-6030(01)00398-7.CrossRefGoogle Scholar
Zhang, X. Wang, L. Zhou, X. Ni, Z. Xia, S., Investigation into the enhancement of property and the difference of mechanism onto visible light degradation of gaseous toluene catalyzed by ZnAl layered double hydroxides before and after Au supporting ACS Sustainable Chemistry & Engineering. 2018 6 1339513407 10.1021/acssuschemeng.8b03186.CrossRefGoogle Scholar
Zhao, Y. F. Zhang, S. Li, B. Yan, H. He, S. Tian, L. Duan, X., A Family of Visible-Light Responsive Photocatalysts Obtained by Dispersing CrO6 Octahedra into a Hydrotalcite Matrix Chemistry -A European Journal 2011 17 1317513181 10.1002/chem.201101874.CrossRefGoogle ScholarPubMed
Zhou, C. H., Emerging trends and challenges in synthetic clay-based materials and layered double hydroxides Applied Clay Science 2010 48 14 10.1016/j.clay.2009.12.018.CrossRefGoogle Scholar
Zhou, Chun Hui Keeling, John, Fundamental and applied research on clay minerals: From climate and environment to nanotechnology Applied Clay Science 2013 74 39 10.1016/j.clay.2013.02.013.CrossRefGoogle Scholar
Zhou, C. H. Li, Z. Z. Ai, Q. W. Tian, H. C. Hong, P. H., Current fundamental and applied research into clay minerals in china Applied Clay Science 2016 119 37 10.1016/j.clay.2015.07.043.CrossRefGoogle Scholar
Figure 0

Fig. 1 XRD patterns of Mg3Cr-CO3-LDHs (a), Co3Cr-CO3-LDHs (b), Ni3Cr-CO3-LDHs (c), Cu3Cr-CO3-LDHs (d), and Zn3Cr-CO3-LDHs (e)

Figure 1

Fig. 2 FTIR patterns of Mg3Cr-CO3-LDHs (a), Co3Cr-CO3-LDHs (b), Ni3Cr-CO3-LDHs (c), Cu3Cr-CO3-LDHs (d), and Zn3Cr-CO3-LDHs (e)

Figure 2

Fig. 3 TG curves of of M3Cr-CO3-LDHs (a), and DTA curves of M3Cr-CO3-LDHs (b)

Figure 3

Fig. 4 UV-Vis DRS patterns of Mg3Cr-CO3-LDHs (a), Co3Cr-CO3-LDHs (b), Ni3Cr-CO3-LDHs (c), Cu3Cr-CO3-LDHs (d), and Zn3Cr-CO3-LDHs (e)

Figure 4

Fig. 5 Photocatalytic degradation of MB under various conditions

Figure 5

Fig. 6 Catalyst recycling study of ZnCr-CO3-LDHs for photocatalytic degradation of MB

Figure 6

Fig. 7 XRD patterns of ZnCr-CO3-LDHs after various cycle times

Figure 7

Fig. 8 Effect of catalyst types on degradation of MB

Figure 8

Fig. 9 UV-Vis absorption spectra of MB with different reaction times in the presence of ZnCr-CO3-LDHs/H2O2 under visible light irradiation.

Figure 9

Fig. 10 Effect of various scavengers on degradation of MB

Figure 10

Fig. 11 Possible mechanism of photocatalytic degradation of MB using ZnCr-CO3-LDHs