Hostname: page-component-cd9895bd7-jkksz Total loading time: 0 Render date: 2024-12-27T14:18:16.294Z Has data issue: false hasContentIssue false

Laser-induced microstructures on silicon for laser-driven acceleration experiments

Published online by Cambridge University Press:  19 June 2017

Tina Ebert*
Affiliation:
Department of Nuclear Physics, TU Darmstadt, Germany
Nico W. Neumann
Affiliation:
Department of Nuclear Physics, TU Darmstadt, Germany
Torsten Abel
Affiliation:
Department of Nuclear Physics, TU Darmstadt, Germany
Gabriel Schaumann
Affiliation:
Department of Nuclear Physics, TU Darmstadt, Germany
Markus Roth
Affiliation:
Department of Nuclear Physics, TU Darmstadt, Germany
*
Correspondence to: T. Ebert Email: tebert@ikp.tu-darmstadt.de

Abstract

Ultrashort laser pulses are used to create surface structures on thin ($25~\unicode[STIX]{x03BC}\text{m}$) silicon (Si) wafers. Scanning the wafer with a galvanometric mirror system creates large homogeneously structured areas. The variety of structure shapes that can be generated with this method is exemplified by the analysis of shape, height and distance of structures created in the ambient media air and isopropanol. A study of the correlation between structure height and remaining wafer thickness is presented. The comparatively easy manufacturing technique and the structure variety that allows for custom-tailored targets show great potential for high repetition rate ion acceleration experiments.

Type
Research Article
Creative Commons
Creative Common License - CCCreative Common License - BY
This is an Open Access article, distributed under the terms of the Creative Commons Attribution licence (http://creativecommons.org/licenses/by/4.0/), which permits unrestricted re-use, distribution, and reproduction in any medium, provided the original work is properly cited.
Copyright
© The Author(s) 2017

1 Introduction

Over the last decade, the interaction of high-intensity laser fields with thin solid targets has attracted a great deal of attention due to its wide field of application. During the interaction process high-energy electrons are emitted[Reference Snavely, Key, Hatchett, Cowan, Roth, Phillips, Stoyer, Henry, Sangster, Singh, Wilks, MacKinnon, Offenberger, Pennington, Yasuike, Langdon, Lasinski, Johnson, Perry and Campbell1]. These ‘hot electrons’ also give rise to an emission of x-rays[Reference Kmetec, Gordon, Macklin, Lemoff, Brown and Harris2] and high-energy ion beams[Reference Hatchett, Brown, Cowan, Henry, Johnson, Key, Koch, Langdon, Lasinski, Lee, Mackinnon, Pennington, Perry, Phillips, Roth, Sangster, Singh, Snavely, Stoyer, Wilks and Yasuike3, Reference Roth and Schollmeier4]. One of the underlying mechanisms is the target normal sheath acceleration (TNSA), where the heated electrons lead to a charge separation that creates strong electrostatic fields accelerating the ions[Reference Wilks, Langdon, Cowan, Roth, Singh, Hatchett, Key, Pennington, MacKinnon and Snavely5]. To increase the number and energy of the hot electrons much effort has been spent on the improvement of the conversion efficiency of laser energy into hot electron energy. To foster conversion efficiency, not only the laser parameters, i.e., laser intensity, pulse duration and energy, but also the target design can be tuned[Reference Jiang, Krygier, Schumacher, Akli and Freeman6Reference Habara, Honda, Katayama, Sakagami, Nagai and Tanaka8].

Recent theoretical studies have shown that modifications of the front surface of the targets improve both laser absorption, hence an increased number and energy of the hot electrons, and collimation of the emitted ion beam by guiding effects[Reference Jiang, Krygier, Schumacher, Akli and Freeman6, Reference Andreev, Kumar, Platonov and Pukhov7]. Supplementary experimental work with nano-wire[Reference Habara, Honda, Katayama, Sakagami, Nagai and Tanaka8] and nano-brush[Reference Zhao, Cao, Cao, Wang, Huang, Jiang, He, Wu, Zhu, Dong, Ding, Zhang, Gu, Yu and He9] targets confirm these results and also show a suppressed plasma expansion on the front side of the target.

There exist various methods to create these surface structures such as electrochemical etching[Reference Zhuang and Edgar10], microcontact printing[Reference Wilbur, Kumar, Kim and Whitesides11], optical[Reference Mack12] and electron beam lithography[Reference Tseng, Chen, Chen and Ma13], chemical vapor deposition[Reference Kong, Cassell and Dai14] or short-pulse laser treatment[Reference Liu, Coxon, Peters, Hoex, Cole and Fray15, Reference Tull, Carey, Mazur, McDonald and Yalisove16]. The latter has multiple advantages, including the possibility to create a wide range of structure variations. Once the laser system is set up, this method is also comparatively time- and cost-efficient. Along with different metals like Cu and Al the processing of crystalline silicon (Si) samples was studied intensively in the last two decades[Reference Her, Finlay, Wu, Deliwala and Mazur17Reference Nayak and Gupta19]. Here, a flat Si surface is processed with a femtosecond-pulsed laser resulting in conical spikes of different height, distance and shape depending on the laser fluence, the number of incident laser pulses, the wavelength, the pulse duration and the ambient medium. It is commonly assumed that these structures are generated by an interference of the incoming and the scattered light and the excitation of surface plasmon-polaritons. The laser–solid interaction causes the electrons and the lattice to heat rapidly. Depending on the laser pulse intensity this results in melting and rapid solidification of the surface or in an ablation of surface atoms. Even though the underlying processes are not completely understood yet, the method can be applied and the influences of the different parameters can be analyzed. Respective studies showed that processing in air or vacuum creates blunt spikes on a micrometer scale, whereas ambient gases containing sulfur result in sharper spikes[Reference Sheehy, Winston, Carey, Friend and Mazur20]. If liquid media like water or alcohol are chosen, the structures are smaller and smoother[Reference Liu, Chen, Wang, Yang, Bian, Si and Hou21]. This wide variety can be exploited to create custom-shaped structures for laser acceleration experiments.

So far, microstructured Si has found its main application in the solar industry because it enhances the light absorption in the complete spectrum emitted by the Sun[Reference Liu, Coxon, Peters, Hoex, Cole and Fray15]. The higher absorption is explained to be due to an increased surface area, the high aspect ratioof the cones trapping the light and a modified band gap as a result of doping the surface with ambient atoms. But Si is also a desirable choice as target material for laser acceleration experiments because it is easily available, comparatively cheap and easy to handle. The amount of fabricated targets can be upscaled without much effort once the parameters are set. Therefore, the technique is suitable for the target production for high repetition laser ion acceleration experiments. In this case, the individual targets would have to be placed on a suitable mount to prevent them from shock damage. If needed, it can be coated with thin layers of different materials like Au or Ni on both sides (flat and structured).

This paper presents a comparative study of short-pulse laser structured Si in air and alcohol with special focus on the different shapes and heights of the cones. To our knowledge, it is the first time that this was done on very thin Si wafers (approx. $25~\unicode[STIX]{x03BC}\text{m}$ ) to be employed in laser-driven acceleration experiments. The results demonstrate the enormous potential of short-pulse laser structuring for custom-tailored solid targets.

2 Experimental setup

The microstructuring experiments described in this paper were conducted using an amplified Ti:sapphire laser system (KMLabs Inc.) with a central wavelength of 800 nm, a pulse duration of 100 fs and a repetition rate of 5 kHz. The power was adjusted by a combination of a waveplate and a polarizer and could be varied continuously in between 50 and 800 mW. The laser had a spatially Gaussian beam shape and was linearly polarized.

For all experiments crystalline Si samples with a thickness of $25~\unicode[STIX]{x03BC}\text{m}$ and a $\langle 100\rangle$ surface orientation were used. To simplify the handling, these thin membranes were enclosed by a thicker frame ( $600~\unicode[STIX]{x03BC}\text{m}$ ) and attached to a scanning electron microscope (SEM) holder pin (Figure 1). This pin was then placed in one of the processing chambers, which vary for different ambient media.

Figure 1. Sectional view of the Si wafer attached to an SEM pin for processing.

Figure 2 shows schematics of the two different processing chambers. In both setups the laser enters the chamber from above and impinges perpendicular on the Si sample surface. For microstructuring in air [Figure 2(a)], an open chamber with no extra supplements was chosen. To keep a constant filling level while microstructuring in fluid ambient media, a plate capacitor was added [Figure 2(b)]. A continuous capacity measurement provides information about the variation of the fluid amount during the process, which allows to keep the level constant.

Figure 2. The setups for the two employed ambient media. Setup (a) was used for processing in air and setup (b) for processing in fluid ambient media. The latter has an additional plate capacitor to monitor the fluid level.

To create larger structured areas the sample was scanned by the laser using a galvanometric two-mirror system. The wafers crystal orientation relative to the scan direction has no influence on the structures, so the initial positioning can be arbitrary. The velocity and step size depend on the ambient medium. Typically, the velocity was varied in between $0.5$ and $2~\text{mm}/\text{s}$ and the optimal step distance was in between 40% and 70% of the focal spot diameter. The position of the best focus was determined by varying the distance between focusing lens (300 mm focal length) and sample surface, thereby identifying the smallest focal spot size on the surface. For the structuring process this best focus was then placed slightly below the crystalline Si surface to prevent a plasma ignition before the laser hits the surface. With a focal spot size of $(70\pm 5)~\unicode[STIX]{x03BC}\text{m}$ the laser fluence at the sample surface could be tuned in between $4$ and $10~\text{kJ}/\text{m}^{2}$ . All samples were characterized using images taken by an SEM (Phillips XL30 FEG) with different angles.

3 Results

The galvanometric mirror system is used to structure large areas by scanning the surface with the laser focus. A typical size of such a rectangular area is $1~\text{mm}\times 1~\text{mm}$ . The laser scans the probe line by line with a distance $\unicode[STIX]{x0394}d$ between the lines. To achieve a high homogeneity this distance $\unicode[STIX]{x0394}d$ has to be chosen carefully, depending on the laser focus size and the ambient medium. The number of pulses that hit one spot at the surface can be varied by altering the speed or the number of scans. To increase the homogeneity the scanning direction is rotated by an angle $\unicode[STIX]{x0394}\unicode[STIX]{x1D6FC}$ after a full scan of the area, as can be seen in Figure 3. The number of rotations depends on the desired total number of pulses.

The result of this scanning procedure is a homogeneously structured target surface as can be seen in Figure 4. Here, the distance was set to $\unicode[STIX]{x0394}d=40~\unicode[STIX]{x03BC}\text{m}$ while having a focus size of $70~\unicode[STIX]{x03BC}\text{m}$ . The overlap has to be determined experimentally, since the employed focal camera measures the $1/\text{e}^{2}$ spot size, but the line width on the Si surface is influenced by the melting threshold of the material and therefore varies with intensity. If the distance is smaller than the optimum, the large overlap results in pile ups in between the lines. In case the distance is wider, unstructured gaps appear between the lines where the fluence was not high enough to create structures.

Figure 3. Schematic showing the rotation of the laser scanning raster used to create more homogeneous structures.

Figure 4. Si target structured in isopropanol with 1400 pulses at a fluence of $5.7~\text{kJ}/\text{m}^{2}$ viewed from above with a 1500 $\times$ magnification.

Figure 5. Comparison of the structure shapes resulting from different ambient media. The structures in the left column (images (a) and (c)) were created in air ( $8.6~\text{kJ}/\text{m}^{2}$ , 450 pulses) whereas the cones displayed in the right column (images (b) and (d)) were generated in isopropanol ( $5.7~\text{kJ}/\text{m}^{2}$ , 1400 pulses). The top row (images (a) and (b)) is viewed from above ( $0^{\circ }$ ) while the bottom row (images (c) and (d)) is viewed from the side ( $45^{\circ }$ ).

Depending on the ambient medium used during the structuring process the structures have a different shape and size. Figure 5 shows structures generated in air (left column) and in liquid isopropanol (right column). The structures generated in air have a height of approximately $15~\unicode[STIX]{x03BC}\text{m}$ and are therefore larger than the ones created in isopropanol, which are approximately $4~\unicode[STIX]{x03BC}\text{m}$ tall.

The top row of Figure 5 is viewed from above and shows that the structures created in air have an almost round base, whereas the bases of the structures generated in isopropanol are clearly more angular. Also, the isopropanol structures are separated by a rift of constant width unlike the air structures, that are more disordered. The difference in size also appears in the average distance between the structures which is about $10~\unicode[STIX]{x03BC}\text{m}$ in air and about $3~\unicode[STIX]{x03BC}\text{m}$ in isopropanol.

A side view is displayed in the bottom row of Figure 5. The images were taken under a viewing angle of $45^{\circ }$ . The structures created in air look needle-like with a steep slope whereas the isopropanol structures are more cone-like with broader slopes. The needles are covered with a light fluff and the cones with small beads. This might be explained by the phases of the media which have different heat conduction properties.

Figure 6. Sketch of the target buildup defining the three basic dimensions $d$ , $b$ and $s$ , describing the cone distance, the base and the structure height, respectively.

Besides studying the shape variation in different ambient media the correlation of structure height and remaining substrate thickness was examined, which is of special interest for thin targets used in the scope of laser-induced particle acceleration. Figure 6 shows a sketch of the target buildup with the definitions for the structure height $s$ and the base height $b$ .

Figure 7. Si wafers processed in liquid isopropanol from an approximate $90^{\circ }$ degree side view. The number of pulses were (a) 700, (b) 1400, (c) 1750 and (d) 2100 respectively, with a constant rotation angle of $\unicode[STIX]{x1D6E5}\unicode[STIX]{x1D6FC}=45^{\circ }$ . The laser fluence of $5.7~\text{kJ}/\text{m}^{2}$ was kept the same.

Figure 8. Correlation of remaining substrate thickness $b$ and structure height $s$ for different numbers of pulses. The laser fluence of $5.7~\text{kJ}/\text{m}^{2}$ and the rotation angle of $\unicode[STIX]{x1D6E5}\unicode[STIX]{x1D6FC}=45^{\circ }$ were kept constant, as well as the ambient medium, which was isopropanol in all cases.

For this study the Si wafer was scanned in liquid isopropanol with a laser fluence of $5.7~\text{kJ}/\text{m}^{2}$ with 700, 1400, 1750 and 2100 pulses. This meant 2, 4, 5 and 6 rotations of the scanning direction with a rotation angle of $\unicode[STIX]{x1D6E5}\unicode[STIX]{x1D6FC}=45^{\circ }$ , respectively, since one full scan attributes 350 pulses. Figure 7 shows $90^{\circ }$ side views of the four steps. Parts of the structured target area broke in the sixth rotation when 2100 pulses were applied. The reason for that is that there is almost no base left as can be seen in Figure 7(d). The values for structure and base heights are plotted in Figure 8. With increasing number of pulses the structure height increases whereas the base height decreases. Both correlations are nonlinear. If taller cones or needles with a thicker base height are required a different initial wafer thickness needs to be chosen. The results presented in this paper are summarized in Table 1.

Table 1. Approximate dimensions of structured Si regarding the height and distance of the cones in different ambient media.

4 Summary

In summary, thin Si wafers are microstructured using femtosecond laser pulses in both air and isopropanol. The different characteristics of these structures are discussed. Although the spatial distribution of the structures is random, the shapes, heights and distances can be controlled by choosing the right parameter set of laser fluence, number of incident pulses and ambient medium. Furthermore, the ratio of structure height and remaining substrate thickness can be influenced. The processing method can be easily applied to large areas and is shown to create a homogeneously structured surface.

Altogether, laser-induced surface structures on thin Si substrates show a great potential as targets for high repetition rate ion acceleration experiments.

Acknowledgements

This work received financial support by the DFG in the framework of the Excellence Initiative, Darmstadt Graduate School of Excellence Energy Science and Engineering (GSC 1070). The authors thank the target laboratory of the Nuclear Physics Department, TU Darmstadt, for their support.

References

Snavely, R. A. Key, M. H. Hatchett, S. P. Cowan, T. E. Roth, M. Phillips, T. W. Stoyer, M. A. Henry, E. A. Sangster, T. C. Singh, M. S. Wilks, S. C. MacKinnon, A. Offenberger, A. Pennington, D. M. Yasuike, K. Langdon, A. B. Lasinski, B. F. Johnson, J. Perry, M. D. and Campbell, E. M. Phys. Rev. Lett. 85, 14 (2000).Google Scholar
Kmetec, J. D. Gordon, C. L. Macklin, J. J. Lemoff, B. E. Brown, G. S. and Harris, S. E. Phys. Rev. Lett. 68, 10 (1992).Google Scholar
Hatchett, S. P. Brown, C. G. Cowan, T. E. Henry, E. A. Johnson, J. S. Key, M. H. Koch, J. A. Langdon, A. B. Lasinski, B. F. Lee, R. W. Mackinnon, A. J. Pennington, D. M. Perry, M. D. Phillips, T. W. Roth, M. Sangster, T. C. Singh, M. S. Snavely, R. A. Stoyer, M. A. Wilks, S. C. and Yasuike, K. Phys. Plasmas 7, 2076 (2000).CrossRefGoogle Scholar
Roth, M. and Schollmeier, M. CERN Yellow Reports 1, 231 (2016).Google Scholar
Wilks, S. C. Langdon, A. B. Cowan, T. E. Roth, M. Singh, M. Hatchett, S. Key, M. H. Pennington, D. MacKinnon, A. and Snavely, R. A. Phys. Plasmas 8, 2 (2001).Google Scholar
Jiang, S. Krygier, A. G. Schumacher, D. W. Akli, K. U. and Freeman, R. R. Phys. Rev. E. Stat. Nonlin. Soft Matter Phys. 89, 1 (2014).Google Scholar
Andreev, A. Kumar, N. Platonov, K. and Pukhov, A. Phys. Plasmas 18, 10 (2011).Google Scholar
Habara, H. Honda, S. Katayama, M. Sakagami, H. Nagai, K. and Tanaka, K. A. Phys. Plasmas 23, 6 (2016).Google Scholar
Zhao, Z. Cao, L. Cao, L. Wang, J. Huang, W. Jiang, W. He, Y. Wu, Y. Zhu, B. Dong, K. Ding, Y. Zhang, B. Gu, Y. Yu, M. Y. and He, X. T. Phys. Plasmas 17, 12 (2010).Google Scholar
Zhuang, D. and Edgar, J. H. Mater. Sci. Eng. R Reports 48, 1 (2005).Google Scholar
Wilbur, J. L. Kumar, A. Kim, E. and Whitesides, G. M. Adv. Mater. 6, 7 (1994).Google Scholar
Mack, C. Fundamental Principles of Optical Litography: The Science of Microfabrication (John Wiley & Sons, 2008).Google Scholar
Tseng, A. A. Chen, K. Chen, C. D. and Ma, K. J. IEEE Trans. Electron. Packag. Manuf. 26, 2 (2003).Google Scholar
Kong, J. Cassell, A. M. and Dai, H. Chem. Phys. Lett. 292, 4 (1998).Google Scholar
Liu, X. Coxon, P. R. Peters, M. Hoex, B. Cole, J. M. and Fray, D. J. Energy Environ. Sci. 7, 10 (2014).Google Scholar
Tull, B. R. Carey, J. E. Mazur, E. McDonald, J. P. and Yalisove, S. M. MRS Bull. 31, 8 (2006).Google Scholar
Her, T. Finlay, R. J. Wu, C. Deliwala, S. and Mazur, E. Appl. Phys. Lett. 73, 12 (1998).Google Scholar
Huang, M. Zhao, F. Cheng, Y. Xu, N. and Xu, Z. ACS Nano 3, 12 (2009).Google Scholar
Nayak, B. K. and Gupta, M. C. Opt. Lasers Eng. 48, 10 (2010).Google Scholar
Sheehy, M. A. Winston, L. Carey, J. E. Friend, C. M. and Mazur, E. Chem. Mater. 17, 14 (2005).Google Scholar
Liu, H. Chen, F. Wang, X. Yang, Q. Bian, H. Si, J. and Hou, X. Thin Solid Films 518, 18 (2010).Google Scholar
Figure 0

Figure 1. Sectional view of the Si wafer attached to an SEM pin for processing.

Figure 1

Figure 2. The setups for the two employed ambient media. Setup (a) was used for processing in air and setup (b) for processing in fluid ambient media. The latter has an additional plate capacitor to monitor the fluid level.

Figure 2

Figure 3. Schematic showing the rotation of the laser scanning raster used to create more homogeneous structures.

Figure 3

Figure 4. Si target structured in isopropanol with 1400 pulses at a fluence of $5.7~\text{kJ}/\text{m}^{2}$ viewed from above with a 1500 $\times$ magnification.

Figure 4

Figure 5. Comparison of the structure shapes resulting from different ambient media. The structures in the left column (images (a) and (c)) were created in air ($8.6~\text{kJ}/\text{m}^{2}$, 450 pulses) whereas the cones displayed in the right column (images (b) and (d)) were generated in isopropanol ($5.7~\text{kJ}/\text{m}^{2}$, 1400 pulses). The top row (images (a) and (b)) is viewed from above ($0^{\circ }$) while the bottom row (images (c) and (d)) is viewed from the side ($45^{\circ }$).

Figure 5

Figure 6. Sketch of the target buildup defining the three basic dimensions $d$, $b$ and $s$, describing the cone distance, the base and the structure height, respectively.

Figure 6

Figure 7. Si wafers processed in liquid isopropanol from an approximate $90^{\circ }$ degree side view. The number of pulses were (a) 700, (b) 1400, (c) 1750 and (d) 2100 respectively, with a constant rotation angle of $\unicode[STIX]{x1D6E5}\unicode[STIX]{x1D6FC}=45^{\circ }$. The laser fluence of $5.7~\text{kJ}/\text{m}^{2}$ was kept the same.

Figure 7

Figure 8. Correlation of remaining substrate thickness $b$ and structure height $s$ for different numbers of pulses. The laser fluence of $5.7~\text{kJ}/\text{m}^{2}$ and the rotation angle of $\unicode[STIX]{x1D6E5}\unicode[STIX]{x1D6FC}=45^{\circ }$ were kept constant, as well as the ambient medium, which was isopropanol in all cases.

Figure 8

Table 1. Approximate dimensions of structured Si regarding the height and distance of the cones in different ambient media.